Preparation method of slow-release carbon source for enhancing nitrogen removal by denitrification
The preparation of sustained release carbon sources by combining modified gasification slag with modified polylactic acid copolymers has solved the problems of high cost of existing carbon sources and unstable sustained release, achieved stable sustained release and efficient nitrogen removal effects, and improved microbial Utilization and economical sewage treatment.
Patent Information
- Application Number
- CN202411239472.2
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-05
- Publication Date
- 2024-12-06
AI Technical Summary
The existing carbon sources are costly in wastewater treatment, excessive dissolution leads to secondary pollution, and are unstable in sustained release, low microbial utilization, making it difficult to achieve both economical and high nitrogen removal performance.
The modified gasification slag and modified polylactic acid copolymer are combined to prepare a sustained release carbon source. The gasification slag is modified by pickling, calcining and guanidine oligomer, and polymerized with functional monomers and crosslinking agents to form a stable Nitrogenation-delayed carbon source.
It has achieved stable and slowed release of carbon sources, improved microbial utilization and biological denitrification effect, reduced sewage treatment costs, and reduced secondary pollution risks.
Smart Images

Figure BDA0005028798090000071 
Figure BDA0005028798090000081 
Figure BDA0005028798090000082
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of water treatment, and in particular relates to a method for preparing a slow-release carbon source for enhanced denitrification and denitrification. Background Art
[0002] Nitrate pollution is a serious environmental problem that affects the quality of surface and groundwater, threatening human and ecosystem health. Excessive nitrogen emissions not only lead to eutrophication, but may also indirectly cause health risks such as methemoglobinemia, gastrointestinal cancer, adverse pregnancy phenomena, thyroid disease, and neural tube defects.
[0003] There are many methods for removing nitrates, such as physical and chemical methods (reverse osmosis, electrodialysis, ion exchange, chemical denitrification, etc.) and biological methods, such as autotrophic or heterotrophic denitrification and nitrate reduction to ammonium. Among them, microbial heterotrophic denitrification is currently the most economical and effective method for wastewater denitrification. Microbial heterotrophic denitrification is a process in which denitrifying bacteria use nitrate reductase (NR), nitrite reductase (NIR), nitric oxide reductase (NOR), and nitrous oxide reductase (NOS) to reduce NO 3 Reduced to NO 2 、NO、N 2 O, eventually reduced to N 2 The above process requires sufficient carbon source to provide electrons for denitrifying bacteria.
[0004] At present, the commonly used traditional added carbon sources include sodium acetate, glucose, methanol, etc. These carbon sources are expensive, and their cost accounts for more than 70% of the total cost of wastewater treatment agents; at the same time, this type of carbon source is soluble in excessive addition, which is easy to cause secondary pollution and lead to high effluent COD. As a new type of solid carbon source with a wide source, low price and the ability to slowly release organic carbon, slow-release carbon sources have been very popular in research in recent years. The use of natural cellulose carbon sources (natural carbon sources) and synthetic biodegradable carbon sources (synthetic carbon sources) as denitrification electron donors can enhance the denitrification effect of the system. However, this type of slow-release carbon source material still has the problems of unstable carbon release and cycle, difficult degradation, and poor microbial utilization. Therefore, there is an urgent need to find an alternative carbon source that is both economical and has high denitrification performance. Summary of the invention
[0005] The primary purpose of the present invention is to provide a method for preparing a slow-release carbon source for enhanced denitrification and denitrification, so as to achieve stable release of the carbon source and have the advantages of being biodegradable, having a long cycle and being eco-friendly.
[0006] To this end, the present invention provides the following technical solutions.
[0007] One aspect of the present invention provides a method for preparing a slow-release carbon source for enhanced denitrification and denitrification, comprising the following steps:
[0008] The gasified slag is immersed in 0.1-0.3 mol / L acid solution at 40-60°C and 200-400 rpm for 1-3 hours of stirring to obtain acid-washed gasified slag; the acid-washed gasified slag is calcined at 800-1200°C for 4-10 hours to obtain calcined gasified slag; the calcined gasified slag is cooled to room temperature and immersed in 40-60 wt% guanidine oligomer solution, and then epichlorohydrin is added and stirred for 4-8 hours, and then the gasified slag is taken out, washed and dried to obtain modified gasified slag;
[0009] Polylactic acid is mixed with 0.1-0.3 mol / L alkali solution in a mass volume ratio of 1 g: 30-100 mL and stirred thoroughly to form a uniform solution, and then functional monomers and initiators are added to the obtained solution and stirred continuously at 30-100° C. for 1-5 hours, and then modified gasified slag and a cross-linking agent are added and stirred continuously for 1-2 hours. After the reaction is completed, the solution is cooled to room temperature and filtered, and the obtained solid product is washed, freeze-dried in vacuum, and then granulated to obtain the denitrification slow-release carbon source with a particle size of 1-5 mm.
[0010] In a preferred embodiment of the present invention, the acid is an inorganic acid or an organic acid, the inorganic acid includes at least one of hydrochloric acid, nitric acid, phosphoric acid, and boric acid, and the organic acid includes at least one of acetic acid, oxalic acid, malic acid, citric acid, and tartaric acid.
[0011] In a preferred embodiment of the present invention, the calcination is a programmed calcination, and the specific process is: first, the temperature is increased to 400-600°C at a heating rate of 1-5°C / min and kept warm for 20-40 minutes, then the temperature is increased to 800-1200°C at a heating rate of 5-10°C / min and kept warm for 4-10 hours.
[0012] In a preferred embodiment of the present invention, the guanidine oligomer is obtained by mixing a polyamine small molecule and a guanidine salt in a mass ratio of 1:1.5 to 3 and stirring at 150 to 200° C. until the mixture is completely fused.
[0013] In a preferred embodiment of the present invention, the polyamine small molecule includes at least one of 2,2'-(diethoxy)diethylamine, trimethylhexanediamine, diethylenetriamine, triethylenetetramine, and tetraethylenepentamine.
[0014] In a preferred embodiment of the present invention, the guanidine salt includes at least one of guanidine hydrochloride, guanidine nitrate, aminoguanidine hydrochloride, triaminoguanidine hydrochloride, and biguanide hydrochloride.
[0015] In a preferred embodiment of the present invention, the amount of epichlorohydrin added is 0.03 to 0.06 times the mass of the gasified slag.
[0016] In a preferred embodiment of the present invention, the functional monomer is selected from any one of N,N-dimethyl-N-acryloylethoxy-N-(3-sulfopropyl)-ammonium betaine, N,N-dimethyl-N-acrylamidopropyl-N-(2-carboxymethyl)-ammonium betaine, N,N-dimethyl-N-acrylamidopropyl-N-(3-sulfopropyl)-ammonium betaine, N,N-dimethyl-N-acrylamidopropyl-N-(2-carboxymethyl)-ammonium betaine, and 2-(methylthio)ethylmethacryloyl-S-(sulfopropyl)-sulfonium betaine.
[0017] In a preferred embodiment of the present invention, the added amount of the functional monomer is 1 to 3 times the mass of the polylactic acid.
[0018] In a preferred embodiment of the present invention, the initiator is selected from any one of benzoyl peroxide, lauroyl peroxide, azobisisobutyronitrile and ammonium persulfate.
[0019] In a preferred embodiment of the present invention, the added amount of the initiator is 0.3-0.5% of the mass of the functional monomer.
[0020] In a preferred embodiment of the present invention, the added amount of the modified gasified slag is 0.5 to 1 times the mass of the polylactic acid.
[0021] In a preferred embodiment of the present invention, the cross-linking agent is selected from any one of catechol, hydroquinone, and resorcinol, or a mixture of two or more thereof.
[0022] In a preferred embodiment of the present invention, the amount of the cross-linking agent added is 0.01 to 0.05 times the mass of the polylactic acid.
[0023] By means of the above technical scheme, the present invention has at least the following advantages: the slow-release carbon source of the present invention is obtained by compounding modified gasification slag and modified polylactic acid copolymer, wherein the modified gasification slag is obtained by acid washing, calcination and modification with guanidine oligomer solution, and the modified polylactic acid is obtained by polymerization and cross-linking of polylactic acid and functional monomers, and both modified substances can be used as carbon source materials. After compounding, the advantages of the two carbon source materials can be fully utilized, which can not only make the carbon source relatively stably and slowly released, but also can be used as a microbial carrier to increase biomass, thereby improving the biological denitrification effect.
[0024] The above description is only an overview of the technical solution of the present invention. In order to more clearly understand the technical means of the present invention and implement it according to the contents of the specification, the preferred embodiments of the present invention are described in detail as follows. DETAILED DESCRIPTION
[0025] In order to make the technical means, creative features, objectives and effects of the present invention easy to understand, the technical solutions in the embodiments of the present invention will be clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0026] Unless otherwise specified, the experimental methods used in the following examples are all conventional methods.
[0027] Unless otherwise specified, the gasification slag used in the following embodiments is coal gasification fine slag purchased from Shenmu Hongjing Purification Coal Co., Ltd., and polylactic acid was purchased from Hubei Xinghengye Technology Co., Ltd.; other materials, reagents, etc. can be obtained from commercial channels.
[0028] Embodiment 1:
[0029] The gasified slag was immersed in a 0.2 mol / L hydrochloric acid solution and stirred at 50°C and 300 rpm for 2 hours to obtain the gasified slag after pickling. The gasified slag after pickling was calcined at high temperature. The specific process was as follows: first, the temperature was increased to 500°C at a heating rate of 5°C / min and kept for 30 minutes, and then the temperature was increased to 1000°C at a heating rate of 10°C / min and kept for 7 hours to obtain the calcined gasified slag. The gasified slag cooled to room temperature after calcination was immersed in a 50wt% guanidine oligomer solution (mixed with 2,2'-(diethoxy)diethylamine and guanidine hydrochloride in a mass ratio of 1:2.25 and stirred at 175°C until completely fused), and then epichlorohydrin was added (the amount added was 0.045 times the mass of the gasified slag) and stirred for 6 hours, and then the gasified slag was taken out, washed and dried to obtain the modified gasified slag.
[0030] Polylactic acid was mixed with 0.2 mol / L sodium hydroxide solution in a mass volume ratio of 1 g: 65 mL and stirred thoroughly to form a uniform solution. N, N-dimethyl-N-acryloylethoxy-N-(3-sulfopropyl)-ammonium betaine (the amount added was 2 times the mass of polylactic acid) and azobisisobutyronitrile (the amount added was 0.4% of the mass of N, N-dimethyl-N-acryloylethoxy-N-(3-sulfopropyl)-ammonium betaine) were added to the resulting solution and stirred for 3 h at 65 ° C. Subsequently, modified gasified slag (the amount added was 0.75 times the mass of polylactic acid) and catechol (the amount added was 0.03 times the mass of polylactic acid) were added and stirred for 1.5 h. After the reaction was completed, it was cooled to room temperature and filtered. The obtained solid product was washed, vacuum freeze-dried and granulated to obtain a denitrification slow-release carbon source with a particle size of 3 mm.
[0031] Embodiment 2:
[0032] The gasified slag was immersed in a 0.2 mol / L hydrochloric acid solution and stirred at 50°C and 300 rpm for 2 hours to obtain the gasified slag after pickling. The gasified slag after pickling was calcined at high temperature, and the specific process was as follows: first, the temperature was increased to 500°C at a heating rate of 5°C / min and kept for 30 minutes, and then the temperature was increased to 1000°C at a heating rate of 10°C / min and kept for 7 hours to obtain the calcined gasified slag. The gasified slag cooled to room temperature after calcination was immersed in a 40wt% guanidine oligomer solution (mixed with trimethylhexanediamine and guanidine nitrate in a mass ratio of 1:1.5 and stirred at 200°C until completely fused), and then epichlorohydrin was added (the amount added was 0.06 times the mass of the gasified slag) and stirred for 4 hours, and then the gasified slag was taken out, washed and dried to obtain the modified gasified slag.
[0033] Polylactic acid was mixed with 0.3 mol / L sodium hydroxide solution in a mass volume ratio of 1 g:30 mL and stirred thoroughly to form a uniform solution. Then, N, N-dimethyl-N-acrylamidopropyl-N-(3-sulfopropyl)-ammonium betaine (the amount added was 1 times the mass of polylactic acid) and ammonium persulfate (the amount added was 0.3% of the mass of N, N-dimethyl-N-acrylamidopropyl-N-(3-sulfopropyl)-ammonium betaine) were added to the resulting solution and stirred for 3 h at 75 ° C. Subsequently, modified gasified slag (the amount added was 0.5 times the mass of polylactic acid) and hydroquinone (the amount added was 0.01 times the mass of polylactic acid) were added and stirred for 2 h. After the reaction was completed, it was cooled to room temperature and filtered. The obtained solid product was washed, vacuum freeze-dried and granulated to obtain a denitrification slow-release carbon source with a particle size of 5 mm.
[0034] Embodiment 3:
[0035] The gasified slag was immersed in a 0.2 mol / L hydrochloric acid solution and stirred at 50°C and 300 rpm for 2 hours to obtain the gasified slag after pickling. The gasified slag after pickling was calcined at high temperature, and the specific process was as follows: first, the temperature was increased to 500°C at a heating rate of 5°C / min and kept for 30 minutes, and then the temperature was increased to 1000°C at a heating rate of 10°C / min and kept for 7 hours to obtain the calcined gasified slag. The gasified slag cooled to room temperature after calcination was immersed in a 60wt% guanidine oligomer solution (mixed with diethylenetriamine and triaminoguanidine hydrochloride in a mass ratio of 1:3 and stirred at 150°C until completely fused), and then epichlorohydrin was added (the amount added was 0.03 times the mass of the gasified slag) and stirred for 8 hours, and then the gasified slag was taken out, washed and dried to obtain the modified gasified slag.
[0036] Polylactic acid was mixed with 0.1 mol / L sodium hydroxide solution in a mass volume ratio of 1 g: 100 mL and stirred thoroughly to form a uniform solution. Then, N, N-dimethyl-N-acrylamidopropyl-N-(2-carboxymethyl)-ammonium betaine (the amount added was 3 times the mass of polylactic acid) and lauroyl peroxide (the amount added was 0.5% of the mass of N, N-dimethyl-N-acrylamidopropyl-N-(2-carboxymethyl)-ammonium betaine) were added to the resulting solution and stirred for 3 h at 60 ° C. Subsequently, modified gasified slag (the amount added was 1 times the mass of polylactic acid) and resorcinol (the amount added was 0.05 times the mass of polylactic acid) were added and stirred for 1 h. After the reaction was completed, it was cooled to room temperature and filtered. The obtained solid product was washed, vacuum freeze-dried and granulated to obtain a denitrification slow-release carbon source with a particle size of 1 mm.
[0037] Comparative Example 1:
[0038] The gasified slag was immersed in a 50wt% guanidine oligomer solution (mixed with 2,2'-(diethoxy)diethylamine and guanidine hydrochloride in a mass ratio of 1:2.25 and stirred at 175°C until completely fused), and then epichlorohydrin was added (the amount added was 0.045 times the mass of the gasified slag) and stirred for 6 hours. After that, the gasified slag was taken out, washed and dried to obtain modified gasified slag.
[0039] Polylactic acid was mixed with 0.2 mol / L sodium hydroxide solution in a mass volume ratio of 1 g: 65 mL and stirred thoroughly to form a uniform solution. N, N-dimethyl-N-acryloylethoxy-N-(3-sulfopropyl)-ammonium betaine (the amount added was 2 times the mass of polylactic acid) and azobisisobutyronitrile (the amount added was 0.4% of the mass of N, N-dimethyl-N-acryloylethoxy-N-(3-sulfopropyl)-ammonium betaine) were added to the resulting solution and stirred for 3 h at 65 ° C. Subsequently, modified gasified slag (the amount added was 0.75 times the mass of polylactic acid) and catechol (the amount added was 0.03 times the mass of polylactic acid) were added and stirred for 1.5 h. After the reaction was completed, it was cooled to room temperature and filtered. The obtained solid product was washed, vacuum freeze-dried and granulated to obtain a denitrification slow-release carbon source with a particle size of 3 mm.
[0040] Comparative Example 2:
[0041] The gasified slag was immersed in a 0.2 mol / L hydrochloric acid solution and stirred at 50°C and 300 rpm for 2 hours to obtain the acid-washed gasified slag. The acid-washed gasified slag was calcined at high temperature, and the specific process was: firstly, the temperature was increased to 500°C at a heating rate of 5°C / min and kept for 30 minutes, and then the temperature was increased to 1000°C at a heating rate of 10°C / min and kept for 7 hours to obtain the calcined gasified slag, that is, the modified gasified slag.
[0042] Polylactic acid was mixed with 0.2 mol / L sodium hydroxide solution in a mass volume ratio of 1 g: 65 mL and stirred thoroughly to form a uniform solution. N, N-dimethyl-N-acryloylethoxy-N-(3-sulfopropyl)-ammonium betaine (the amount added was 2 times the mass of polylactic acid) and azobisisobutyronitrile (the amount added was 0.4% of the mass of N, N-dimethyl-N-acryloylethoxy-N-(3-sulfopropyl)-ammonium betaine) were added to the resulting solution and stirred for 3 h at 65 ° C. Subsequently, modified gasified slag (the amount added was 0.75 times the mass of polylactic acid) and catechol (the amount added was 0.03 times the mass of polylactic acid) were added and stirred for 1.5 h. After the reaction was completed, it was cooled to room temperature and filtered. The obtained solid product was washed, vacuum freeze-dried and granulated to obtain a denitrification slow-release carbon source with a particle size of 3 mm.
[0043] Comparative Example 3:
[0044] The gasified slag was immersed in a 0.2 mol / L hydrochloric acid solution and stirred at 50°C and 300 rpm for 2 hours to obtain the gasified slag after pickling. The gasified slag after pickling was calcined at high temperature. The specific process was as follows: first, the temperature was increased to 500°C at a heating rate of 5°C / min and kept for 30 minutes, and then the temperature was increased to 1000°C at a heating rate of 10°C / min and kept for 7 hours to obtain the calcined gasified slag. The gasified slag cooled to room temperature after calcination was immersed in a 50wt% guanidine oligomer solution (mixed with 2,2'-(diethoxy)diethylamine and guanidine hydrochloride in a mass ratio of 1:2.25 and stirred at 175°C until completely fused), and then epichlorohydrin was added (the amount added was 0.045 times the mass of the gasified slag) and stirred for 6 hours, and then the gasified slag was taken out, washed and dried to obtain the modified gasified slag.
[0045] Polylactic acid was mixed with 0.2 mol / L sodium hydroxide solution in a mass-to-volume ratio of 1g:65mL and stirred thoroughly to form a uniform solution. Subsequently, modified gasification slag (the amount added was 0.75 times the mass of polylactic acid) and catechol (the amount added was 0.03 times the mass of polylactic acid) were added and stirring was continued for 1.5h. After the reaction was completed, it was cooled to room temperature and filtered. The solid product was washed, freeze-dried in vacuum and granulated to obtain a denitrification slow-release carbon source with a particle size of 3mm.
[0046] Comparative Example 4:
[0047] The gasified slag was immersed in a 0.2 mol / L hydrochloric acid solution and stirred at 50°C and 300 rpm for 2 hours to obtain the gasified slag after pickling. The gasified slag after pickling was calcined at high temperature. The specific process was as follows: first, the temperature was raised to 500°C at a heating rate of 5°C / min and kept warm for 30 minutes, and then the temperature was raised to 1000°C at a heating rate of 10°C / min and kept warm for 7 hours to obtain the calcined gasified slag. The gasified slag cooled to room temperature after calcination was immersed in a 50wt% guanidine oligomer (mixed with 2,2'-(diethoxy)diethylamine and guanidine hydrochloride in a mass ratio of 1:2.25 and stirred at 175°C until completely fused) solution, and then epichlorohydrin was added (the amount added was 0.045 times the mass of the gasified slag) and stirred for 6 hours, and then the gasified slag was taken out for washing and drying. After screening, the modified gasified slag with a particle size of 3mm was obtained as a denitrification slow-release carbon source.
[0048] Comparative Example 5:
[0049] Polylactic acid was mixed with 0.2 mol / L sodium hydroxide solution in a mass volume ratio of 1 g: 65 mL and stirred thoroughly to form a uniform solution. N, N-dimethyl-N-acryloylethoxy-N-(3-sulfopropyl)-ammonium betaine (the amount added was 2 times the mass of polylactic acid) and azobisisobutyronitrile (the amount added was 0.4% of the mass of N, N-dimethyl-N-acryloylethoxy-N-(3-sulfopropyl)-ammonium betaine) were added to the resulting solution and stirred for 3 h at 65 ° C. Subsequently, catechol (the amount added was 0.03 times the mass of polylactic acid) was added and stirred for 1.5 h. After the reaction was completed, it was cooled to room temperature and filtered. The obtained solid product was washed, freeze-dried in vacuum and granulated to obtain a denitrification slow-release carbon source with a particle size of 3 mm.
[0050] Test example: Effects of different carbon sources on denitrification effect and effluent COD
[0051] Experimental method: A water sample from the anaerobic section of a sewage plant was selected for denitrification test, with a sludge concentration of 2000 mg / L, a total nitrogen of 83 mg / L, and a COD of 185 mg / L. Take 8 1000 mL conical flasks, add 5 g of the carbon source obtained in Examples 1 to 3 and Comparative Examples 1 to 5 to each of the 8 conical flasks, add 500 ml of water sample and stir at the same speed in a stirrer, take out water samples at 12 h, 24 h, 36 h, 48 h, 72 h, 96 h, 120 h, 144 h, and 168 h to measure COD, NO 3 - Indicators were used to investigate the effects of different carbon source components on denitrification effect and effluent COD. The results are shown in Tables 1 and 2.
[0052] Table 1 Total nitrogen removal rate of effluent with different carbon source components
[0053]
[0054]
[0055] Table 2 Effect of different carbon source components on effluent COD removal rate
[0056]
[0057] From the results in Table 1, it can be seen that the denitrification denitrification slow-release carbon sources of Examples 1 to 3 of the present invention have higher denitrification rates and COD removal rates than the denitrification slow-release carbon sources of Comparative Examples 1 to 5. Among them, compared with Example 1, the denitrification effect and COD removal rate of the slow-release carbon sources of Comparative Examples 1 to 5 are significantly reduced, which shows that the modified gasification slag and modified polylactic acid of the present invention can work together to increase the comprehensive effect of the slow-release carbon source.
[0058] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Although the present invention has been disclosed as a preferred embodiment as above, it is not used to limit the present invention. Any technician familiar with this profession can make some changes or modifications to equivalent embodiments of equivalent changes by using the methods and technical contents disclosed above without departing from the scope of the technical solution of the present invention. However, any simple modification, equivalent change and modification made to the above embodiments according to the technical essence of the present invention without departing from the content of the technical solution of the present invention still fall within the scope of the technical solution of the present invention.
Claims
1. A method for preparing a slow-release carbon source for enhanced denitrification and denitrification, characterized in that: The following steps are involved: The gasified slag is immersed in a 0.1-0.3 mol / L acid solution at 40-60°C and 200-400 rpm for 1-3 hours of stirring to obtain acid-washed gasified slag; the acid-washed gasified slag is calcined at 800-1200°C for 4-10 hours to obtain calcined gasified slag; the gasified slag cooled to room temperature after calcination is immersed in a 40-60 wt% guanidine oligomer solution, and then epichlorohydrin is added and stirred for 4-8 hours, and then the gasified slag is taken out, washed and dried to obtain modified gasified slag; Polylactic acid is mixed with 0.1-0.3 mol / L alkali solution in a mass volume ratio of 1 g: 30-100 mL and stirred thoroughly to form a uniform solution, and then functional monomers and initiators are added to the obtained solution and stirred continuously at 30-100° C. for 1-5 hours, and then modified gasified slag and a cross-linking agent are added and stirred continuously for 1-2 hours. After the reaction is completed, it is cooled to room temperature and filtered. The obtained solid product is washed, freeze-dried in vacuum, and then granulated to obtain the denitrification slow-release carbon source with a particle size of 1-5 mm.
2. The method according to claim 1, characterized in that The acid is an inorganic acid or an organic acid. The inorganic acid includes at least one of hydrochloric acid, nitric acid, phosphoric acid, and boric acid. The organic acid includes at least one of acetic acid, oxalic acid, malic acid, citric acid, and tartaric acid.
3. The method according to claim 1, characterized in that The calcination is a programmed calcination, and the specific process is: first, the temperature is increased to 400-600°C at a heating rate of 1-5°C / min and kept at this temperature for 20-40 minutes, and then the temperature is increased to 800-1200°C at a heating rate of 5-10°C / min and kept at this temperature for 4-10 hours.
4. The method according to claim 1, characterized in that: The guanidine oligomer is obtained by mixing a polyamine small molecule and a guanidine salt in a mass ratio of 1:1.5-3 and stirring at 150-200° C. until the mixture is completely fused.
5. The method according to claim 4, characterized in that The polyamine small molecule includes at least one of 2,2'-(diethoxy)diethylamine, trimethylhexanediamine, diethylenetriamine, triethylenetetramine, and tetraethylenepentamine; The guanidine salt includes at least one of guanidine hydrochloride, guanidine nitrate, aminoguanidine hydrochloride, triaminoguanidine hydrochloride, and biguanide hydrochloride.
6. The method according to claim 1, characterized in that The amount of epichlorohydrin added is 0.03 to 0.06 times the mass of the gasified slag.
7. The method according to claim 1, characterized in that The functional monomer is selected from any one of N,N-dimethyl-N-acryloylethoxy-N-(3-sulfopropyl)-ammonium betaine, N,N-dimethyl-N-acrylamidopropyl-N-(2-carboxymethyl)-ammonium betaine, N,N-dimethyl-N-acrylamidopropyl-N-(3-sulfopropyl)-ammonium betaine, N,N-dimethyl-N-acrylamidopropyl-N-(2-carboxymethyl)-ammonium betaine, and 2-(methylthio)ethylmethacryloyl-S-(sulfopropyl)-sulfonium betaine; The added amount of the functional monomer is 1 to 3 times the mass of the polylactic acid.
8. The method according to claim 1, characterized in that The initiator is selected from any one of benzoyl peroxide, lauroyl peroxide, azobisisobutyronitrile and ammonium persulfate; The amount of the initiator added is 0.3-0.5% of the mass of the functional monomer.
9. The method according to claim 1, characterized in that: The added amount of the modified gasified slag is 0.5 to 1 times the mass of the polylactic acid.
10. The method according to claim 1, characterized in that The cross-linking agent is selected from any one of catechol, hydroquinone, and resorcinol, or a mixture of two or more thereof; The added amount of the cross-linking agent is 0.01 to 0.05 times the mass of the polylactic acid.
Citation Information
Patent Citations
Preparation of electrically neutral zwitterion type polyacrylamide flocculant
CN101412785A
Preparation method and application of crosslinked starch, polycaprolactone and polylactic acid mixture
CN102206363A
Petrochemical high-salt wastewater desalting treatment device
CN107758990A
Polylactic acid and lactide blended sustained-release material
CN112552664A
Self-degradable biological membrane filler as well as preparation method and application thereof
CN114590886A