Silicon scale inhibitor and preparation method thereof
By combining the terpolymer and polyepoxysuccinic acid, the silica scale formation and silica scale formation in the prior art are solved by using the synergistic effect of its ether bond, carboxyl group, sulfonic acid group and amide group. Eliminate difficulties and achieve efficient scale resistance at low dosage, extend equipment life and stable operation.
Patent Information
- Application Number
- CN202411425301.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-12
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art has poor scale resistance effect within a low dosage range, making it difficult to effectively prevent the formation and removal of silicon scale in industrial water reuse deep treatment systems, resulting in water production rate and heat exchange of membrane systems, evaporation crystallizers and other equipment. The efficiency decreases and the corrosion of the equipment accelerates.
Silica scale inhibitor prepared from terpolymer and polyepoxysuccinic acid composite, the terpolymer contains ether bonds, carboxyl groups, sulfonic acid groups and amide groups, which increases the concentration of dissolved silicon through synergistic action and inhibits it. The formation of silica scale.
At lower dosage, it significantly improves the scale resistance effect, extends the operating life of the equipment, reduces the waste of water resources and the number of equipment parking times, and ensures the stable operation of the system.
Smart Images

Figure BDA0005081977080000121 
Figure BDA0005081977080000122 
Figure BDA0005081977080000131
Abstract
Description
Technical Field
[0001] The invention relates to the field of water treatment, and in particular to a silicon scale inhibitor and a preparation method thereof. Background Art
[0002] At present, in the deep treatment system of industrial water reuse, due to the continuous circulation and concentration of raw water, Ca 2+ Mg 2+ , Cl - 、SO4 2- 、SiO3 2- The continuous accumulation of plasma often leads to scaling and blockage of the membrane system and evaporator crystallizer, which in turn causes a series of hazards such as a decrease in the water production rate, desalination rate of the membrane system and heat exchange efficiency of the crystallizer evaporator, as well as blockage of the heat exchange tubes and accelerated corrosion of the equipment.
[0003] The scale deposits in water mainly contain components such as calcium carbonate, calcium sulfate, calcium silicate, magnesium carbonate and magnesium silicate. Existing scale inhibitors generally achieve the purpose of scale inhibition by inhibiting the deposition and growth of scale crystals. The carbonate scale and sulfate scale in water are loose in texture and easy to remove, but the formation of silica scale is more complicated, and the formation process is divided into internal and external factors. The internal factor mainly refers to the presence of various forms of silicon in the solution, and the external factor is the precipitation of silica scale under various conditions. When there are various forms of silicon and Ca in the system, 2+ Mg 2+ 、CO3 2- 、SO4 2- Silica scale is more likely to form when the concentration of various ions increases to supersaturation to produce calcium silicate and magnesium silicate precipitation. These already formed tiny particles will become nucleation centers, accelerating the precipitation process and forming hard and dense silica scale. (2) Concentration process: The precipitated scale such as calcium carbonate and magnesium hydroxide formed by concentration can provide nucleation centers for silica scale, thereby promoting the formation of mixed scale. (3) Colloid precipitation: High salt content and the decrease in pH and pressure may cause silica colloid to precipitate, forming amorphous or polymerized silica precipitates. (4) When the pressure of an industrial production device drops suddenly, substances such as silicates are most likely to deposit and form silica scale.
[0004] Once formed, silica scale is difficult to remove and is more harmful to the system. There are two common silica scales in industrial water reuse deep treatment systems: one is amorphous colloidal silica, which mostly exists in the form of molecular aggregation or particle attachment in water; the other is silicate scale, common ones are CaSiO3, MgSiO3, etc., which have a dense structure and hard texture. After formation, they adhere to the membrane surface or evaporation crystallization pipeline and are difficult to remove. They can only be pickled with hydrofluoric acid.
[0005] To prevent the formation of silica scale, on the one hand, the silica content of the influent is reduced as much as possible during the pretreatment process, and on the other hand, the formation of silica scale is reduced or prevented by adding scale inhibitors. Adding scale inhibitors can not only fundamentally slow down scaling, but also effectively save water resources and extend the service life of equipment. At present, amines, carboxylic acids, ethers, sulfonic acid polymers and dendritic macromolecules are mostly used on the market to increase the solubility of silica and reduce scaling. However, the amount added is usually large enough to achieve a good scale inhibition effect, which reduces the economic feasibility to a certain extent. Summary of the invention
[0006] The purpose of the present invention is to overcome the problem that the organic polymer scale inhibitor in the prior art has poor scale inhibition effect within a lower dosage range, and provides a silicon scale inhibitor and a preparation method thereof. The silicon scale inhibitor is obtained by compounding a terpolymer and polyepoxysuccinic acid, and the terpolymer contains an ether bond, a carboxyl group, a sulfonic acid group and an amide group, and has good scale inhibition performance against silicon scale in a water treatment system. The silicon scale inhibitor has good scale inhibition performance at a lower dosage level.
[0007] In order to achieve the above-mentioned object, the first aspect of the present invention provides a silica scale inhibitor, which contains a terpolymer and polyepoxysuccinic acid, wherein the terpolymer includes a first structural unit, a second structural unit and a third structural unit, the first structural unit is provided by polyethylene glycol, the second structural unit is provided by N-tert-butyl acrylamide, and the third structural unit is provided by acrylic acid-2-acrylamide-2-methylpropane sulfonic acid copolymer.
[0008] Preferably, the weight average molecular weight of the terpolymer is 500-20,000, more preferably 800-20,000.
[0009] Preferably, in the terpolymer, the molar ratio of the first structural unit, the second structural unit and the third structural unit is (1-20):(20-200):1, more preferably (1-10):(20-150):1.
[0010] Preferably, the weight average molecular weight of the polyethylene glycol is 200-1500, more preferably 400-1200.
[0011] Preferably, the weight average molecular weight of the acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer is 800-2000, more preferably 1000-2000.
[0012] Preferably, the weight ratio of the terpolymer to the polyepoxysuccinic acid is 1-10:1, more preferably 1-5:1.
[0013] The second aspect of the present invention provides a method for preparing a silicon scale inhibitor, the method comprising the following steps:
[0014] (1) in the presence of an initiator and liquid alkali, polymerizing polyethylene glycol and N-tert-butylacrylamide;
[0015] (2) subjecting the reaction product of step (1) to a polymerization reaction with an acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer;
[0016] (3) Mixing the reaction product of step (2) with polyepoxysuccinic acid.
[0017] Preferably, the molar ratio of the polyethylene glycol, the N-tert-butylacrylamide and the copolymer of 2-acrylamide-2-methylpropanesulfonic acid is (1-20):(20-200):1, more preferably (1-10):(20-150):1.
[0018] Preferably, in step (1), the polymerization reaction conditions include: temperature of 50-150° C., time of 2-8 h, and pH of 8-11.
[0019] Preferably, the weight average molecular weight of the polyethylene glycol is 200-1500, more preferably 500-1200.
[0020] Preferably, the initiator is selected from at least one of ammonium persulfate, ammonium persulfate-sodium bisulfite and sodium bisulfite.
[0021] Preferably, in step (2), the polymerization reaction conditions include: temperature of 20-100° C. and time of 0.5-6 h.
[0022] Preferably, the weight average molecular weight of the acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer is 800-2000, more preferably 1000-1800.
[0023] Preferably, in step (3), the weight ratio of the terpolymer to the polyepoxysuccinic acid is 1-10:1, more preferably 1-5:1.
[0024] In the silicon scale inhibitor described in the present invention, the terpolymer contains an ether bond, a carboxyl group, a sulfonic acid group and an amide group, which can exert the synergistic effect of various functional groups in the water treatment process, increase the concentration of dissolved silicon in the solution, and have a good inhibitory effect on silicon scale. At the same time, the silicon scale inhibitor further improves its scale inhibition performance by compounding the terpolymer with polyepoxysuccinic acid, which is beneficial to achieve stable operation of the system. In the water treatment process, compared with the prior art, the silicon scale inhibitor described in the present invention has a small dosage and a significant scale inhibition effect. Compared with the prior art, it can achieve a good scale inhibition effect at a lower dosage, and the dosing is not affected by the operation of the device, which can ensure the stable operation of the system and reduce device shutdown. DETAILED DESCRIPTION
[0025] The specific embodiments of the present invention are described in detail below. It should be understood that the specific embodiments described herein are only used to illustrate and explain the present invention, and are not used to limit the present invention.
[0026] The endpoints and any values of the ranges disclosed in this article are not limited to the precise ranges or values, and these ranges or values should be understood to include values close to these ranges or values. For numerical ranges, the endpoint values of each range, the endpoint values of each range and the individual point values, and the individual point values can be combined with each other to obtain one or more new numerical ranges, which should be considered as specifically disclosed in this article.
[0027] The silica scale inhibitor of the present invention contains a terpolymer and polyepoxysuccinic acid, wherein the terpolymer includes a first structural unit, a second structural unit and a third structural unit, the first structural unit is provided by polyethylene glycol, the second structural unit is provided by N-tert-butyl acrylamide, and the third structural unit is provided by an acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer.
[0028] In the silica scale inhibitor of the present invention, the weight average molecular weight of the terpolymer can be 500-20000, preferably 800-20000, and more preferably 850-20000. In the present invention, the weight average molecular weight of the polymer is obtained by gel permeation chromatography. In the silica scale inhibitor of the present invention, when the molecular weight of the terpolymer is within the above preferred range (especially within the preferred range), the silica scale inhibitor obtained by compounding the terpolymer has better scale inhibition performance.
[0029] In the silica scale inhibitor of the present invention, in the terpolymer, the molar ratio of the first structural unit, the second structural unit and the third structural unit can be (1-20): (20-200): 1, preferably (1-10): (20-150): 1, and more preferably (1-5): (20-100): 1. In the terpolymer, when the molar ratio of the first structural unit, the second structural unit and the third structural unit is within the above selection range (especially within the preferred range), the silica scale inhibitor obtained by compounding the terpolymer can exert better scale inhibition performance at a lower dosage level.
[0030] In the present invention, the weight average molecular weight of the polyethylene glycol may be 200-1500, preferably 400-1200, and more preferably 500-1200. In the terpolymer of the present invention, when the weight average molecular weight of the polyethylene glycol is within the above-mentioned selection range (especially within the preferred range), the silica scale inhibitor obtained by compounding the terpolymer has better scale inhibition performance.
[0031] In the present invention, the weight average molecular weight of the acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer can be 800-2000, preferably 1000-1800, and more preferably 1200-1800. In the terpolymer of the present invention, when the weight average molecular weight of the acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer is within the above selection range (especially within the preferred range), the silica scale inhibitor obtained by compounding the terpolymer can exert better scale inhibition performance at a lower dosage level.
[0032] In the silica scale inhibitor of the present invention, the weight ratio of the terpolymer to the polyepoxysuccinic acid may be 1-10: 1, preferably 1-5: 1, and more preferably 1-3: 1. In the silica scale inhibitor of the present invention, when the weight ratio of the terpolymer to the polyepoxysuccinic acid is within the above range (especially within the preferred range), the scale inhibition performance of the silica scale inhibitor can be further improved.
[0033] The silica scale inhibitor of the present invention can be prepared by conventional methods in the art. In a preferred embodiment, the silica scale inhibitor is prepared by the following method, which comprises the following steps:
[0034] (1) in the presence of an initiator and liquid alkali, polymerizing polyethylene glycol and N-tert-butylacrylamide;
[0035] (2) subjecting the reaction product of step (1) to a polymerization reaction with an acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer;
[0036] (3) Mixing the reaction product of step (2) with polyepoxysuccinic acid.
[0037] In the method of the present invention, the molar ratio of the polyethylene glycol, the N-tert-butylacrylamide and the copolymer of 2-acrylamide-2-methylpropanesulfonic acid can be (1-20): (20-200): 1, preferably (1-10): (20-150): 1, and more preferably (1-5): (20-100): 1. In the method of the present invention, when the molar ratio of the polyethylene glycol, the N-tert-butylacrylamide and the copolymer of 2-acrylamide-2-methylpropanesulfonic acid is within the above range (especially within the preferred range), the prepared silica scale inhibitor can exert better scale inhibition performance at a lower dosage level.
[0038] In some embodiments, in step (1), the polymerization reaction conditions may include: temperature of 50-150° C., preferably 50-100° C.; time of 2-8 h, preferably 2-5 h; pH of 8-11, preferably 8-10.
[0039] In the method of the present invention, the weight average molecular weight of the polyethylene glycol may be 200-1500, preferably 500-1200, and more preferably 600-1200. In these embodiments, when the weight average molecular weight of the polyethylene glycol is within the above range (especially within the preferred range), the prepared terpolymer has better scale inhibition performance.
[0040] In the present invention, the initiator may be at least one of ammonium persulfate, ammonium persulfate-sodium bisulfite and sodium bisulfite, preferably ammonium persulfate.
[0041] In the present invention, the liquid alkali may be liquid sodium hydroxide.
[0042] In some embodiments, in step (1), the process of polymerizing polyethylene glycol and N-tert-butylacrylamide may also include: mixing deionized water and polyethylene glycol, heating the mixture in a water bath, and then simultaneously adding an initiator, liquid alkali and N-tert-butylacrylamide dropwise to the resulting mixed solution, and reacting after the addition is completed, wherein the addition time is 20-60 minutes.
[0043] In some embodiments, in step (2), the polymerization reaction conditions may include: temperature of 20-100° C., preferably 20-50° C.; time of 0.5-6 h, preferably 1-3 h.
[0044] In the method of the present invention, the weight average molecular weight of the acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer may be 800-2000, preferably 1000-2000, and more preferably 1000-1800. In these embodiments, when the weight average molecular weight of the acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer is within the above range (especially within the preferred range), the prepared terpolymer has better scale inhibition performance.
[0045] In the method of the present invention, in step (3), the weight ratio of the terpolymer to the polyepoxysuccinic acid can be 1-10:1, more preferably 1-5:1. In the method of the present invention, when the weight ratio of the terpolymer to the polyepoxysuccinic acid is within the above range (especially within the preferred range), the prepared silica scale inhibitor can exert better scale inhibition performance at a lower dosage level.
[0046] The silicon scale inhibitor and its preparation method of the present invention are further described by examples. The examples are implemented on the premise of the technical solution of the present invention, and detailed implementation methods and specific operation processes are given, but the protection scope of the present invention is not limited to the following examples.
[0047] The experimental methods in the following examples are all conventional methods in the art unless otherwise specified. The polymers used in the following examples are as follows:
[0048] Polyethylene glycol ( Brand No. 25322-68-3, purchased from Shanghai MacLean Biochemical Technology Co., Ltd.), acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer (active content ≥30.0%, brand No. 40623-75-4, limiting viscosity at 30°C is 0.055-0.100), polyepoxysuccinic acid ( The brand number is 51274-37-4, purchased from Shandong Taihe Science and Technology Co., Ltd.).
[0049] The remaining experimental materials used in the following examples, unless otherwise specified, are commercially available.
[0050] Example 1
[0051] (1) 100 mL of deionized water and 50 mL of polyethylene glycol were added to a three-necked flask in sequence, stirred to mix them evenly, and the three-necked flask was heated in a constant temperature water bath at 85° C. After the temperature of the mixed solution in the three-necked flask reached 85° C., 10 mL of ammonium persulfate, 1 mL of liquid caustic soda and 100 mL of N-tert-butylacrylamide were simultaneously added dropwise to the three-necked flask within 30 min, and then the pH value of the obtained mixed system was adjusted to 8.0, and the reaction was carried out at a constant temperature for 4 h;
[0052] (2) lowering the water bath temperature to 40° C., adding 40 mL of acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer to the product obtained in step (1), and stirring for 2 h to obtain a terpolymer (weight average molecular weight of 850-20000), wherein the molar ratio of the polyethylene glycol, the N-tert-butylacrylamide and the 2-acrylamide-2-methylpropanesulfonic acid copolymer is 3:70:1;
[0053] (3) The terpolymer is prepared into a solution with a concentration of 70 mg / L, and then compounded with polyepoxysuccinic acid with a concentration of 30 mg / L, wherein the molar ratio of the terpolymer to the polyepoxysuccinic acid is 2.3:1, to obtain the silica scale inhibitor of the present invention, calculated as JC-600-1.
[0054] Example 2
[0055] (1) 100 mL of deionized water and 50 mL of polyethylene glycol were added to a three-necked flask in sequence, stirred to mix them evenly, and the three-necked flask was heated in a constant temperature water bath at 85° C. After the temperature of the mixed solution in the three-necked flask reached 85° C., 12 mL of ammonium persulfate, 2 mL of liquid caustic soda and 120 mL of N-tert-butyl acrylamide were simultaneously added dropwise to the three-necked flask within 30 min, and then the pH value of the obtained mixed system was adjusted to 8.5, and the reaction was carried out at a constant temperature for 4 h;
[0056] (2) lowering the water bath temperature to 40° C., adding 40 mL of acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid copolymer to the product obtained in step (1), and stirring for 2 h to obtain a terpolymer (weight average molecular weight of 850-20000), wherein the molar ratio of the polyethylene glycol, the N-tert-butylacrylamide and the 2-acrylamide-2-methylpropanesulfonic acid copolymer is 3:80:1;
[0057] (3) The terpolymer is prepared into a solution with a concentration of 70 mg / L, and then compounded with polyepoxysuccinic acid with a concentration of 30 mg / L, wherein the molar ratio of the terpolymer to the polyepoxysuccinic acid is 2.3:1, to obtain the silica scale inhibitor of the present invention, calculated as JC-600-2.
[0058] Example 3
[0059] (1) 100 mL of deionized water and 60 mL of polyethylene glycol were added to a three-necked flask in sequence, stirred to mix them evenly, and the three-necked flask was heated in a constant temperature water bath at 85° C. After the temperature of the mixed solution in the three-necked flask reached 85° C., 13.5 mL of ammonium persulfate, 1-5 mL of liquid caustic soda and 120 mL of N-tert-butyl acrylamide were simultaneously added dropwise to the three-necked flask within 30 minutes, and then the pH value of the obtained mixed system was adjusted to 8.0-9.0, and the reaction was carried out at a constant temperature for 4 hours;
[0060] (2) lowering the water bath temperature to 40° C., adding 40 mL of acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid copolymer to the product obtained in step (1), and stirring for 2 h to obtain a terpolymer (weight average molecular weight of 850-20000), wherein the molar ratio of the polyethylene glycol, the N-tert-butylacrylamide and the 2-acrylamide-2-methylpropanesulfonic acid copolymer is 4:80:1;
[0061] (3) The terpolymer is prepared into a solution with a concentration of 70 mg / L, and then compounded with polyepoxysuccinic acid with a concentration of 30 mg / L, wherein the molar ratio of the terpolymer to the polyepoxysuccinic acid is 2.3:1, to obtain the silica scale inhibitor of the present invention, calculated as JC-600-3.
[0062] Example 4
[0063] (1) 100 mL of deionized water and 60 mL of polyethylene glycol were added to a three-necked flask in sequence, stirred to mix evenly, and the three-necked flask was heated in a constant temperature water bath at 85° C. After the temperature of the mixed solution in the three-necked flask reached 85° C., 12 mL of ammonium persulfate, 1-5 mL of liquid caustic soda and 130 mL of N-tert-butylacrylamide were simultaneously added dropwise to the three-necked flask within 30 min, and then the pH value of the obtained mixed system was adjusted to 8.0-9.0, and the reaction was carried out at a constant temperature for 4 h;
[0064] (2) lowering the water bath temperature to 40° C., adding 40 mL of acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid copolymer to the product obtained in step (1), and stirring for 2 h to obtain a terpolymer (weight average molecular weight of 850-20000), wherein the molar ratio of the polyethylene glycol, the N-tert-butylacrylamide and the 2-acrylamide-2-methylpropanesulfonic acid copolymer is 4:90:1;
[0065] (3) The terpolymer is prepared into a solution with a concentration of 70 mg / L, and then compounded with polyepoxysuccinic acid with a concentration of 30 mg / L, wherein the molar ratio of the terpolymer to the polyepoxysuccinic acid is 2.3:1, to obtain the silica scale inhibitor of the present invention, calculated as JC-600-4.
[0066] Example 5
[0067] (1) 100 mL of deionized water and 70 mL of polyethylene glycol were added to a three-necked flask in sequence, stirred to mix evenly, and the three-necked flask was heated in a constant temperature water bath at 85° C. After the temperature of the mixed solution in the three-necked flask reached 85° C., 12 mL of ammonium persulfate, 1-5 mL of liquid caustic soda and 130 mL of N-tert-butylacrylamide were simultaneously added dropwise to the three-necked flask within 30 minutes, and then the pH value of the obtained mixed system was adjusted to 8.0-9.0, and the reaction was carried out at a constant temperature for 4 hours;
[0068] (2) lowering the water bath temperature to 40° C., adding 40 mL of acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid copolymer to the product obtained in step (1), and stirring for 2 h to obtain a terpolymer (weight average molecular weight of 850-20000), wherein the molar ratio of the polyethylene glycol, the N-tert-butylacrylamide and the 2-acrylamide-2-methylpropanesulfonic acid copolymer is 5:90:1;
[0069] (3) The terpolymer is prepared into a solution with a concentration of 70 mg / L, and then compounded with polyepoxysuccinic acid with a concentration of 30 mg / L, wherein the molar ratio of the terpolymer to the polyepoxysuccinic acid is 2.3:1, to obtain the silica scale inhibitor of the present invention, calculated as JC-600-5.
[0070] Example 6
[0071] (1) 100 mL of deionized water and 70 mL of polyethylene glycol were added to a three-necked flask in sequence, stirred to mix them evenly, and the three-necked flask was heated in a constant temperature water bath at 85° C. After the temperature of the mixed solution in the three-necked flask reached 85° C., 9 mL of ammonium persulfate, 1-5 mL of liquid caustic soda and 140 mL of N-tert-butylacrylamide were simultaneously added dropwise to the three-necked flask within 30 minutes, and then the pH value of the obtained mixed system was adjusted to 8.0-9.0, and the reaction was carried out at a constant temperature for 4 hours;
[0072] (2) lowering the water bath temperature to 40° C., adding 40 mL of acrylic acid and 2-acrylamide-2-methylpropanesulfonic acid copolymer to the product obtained in step (1), and stirring for 2 h to obtain a terpolymer (weight average molecular weight of 850-20000), wherein the molar ratio of the polyethylene glycol, the N-tert-butylacrylamide and the 2-acrylamide-2-methylpropanesulfonic acid copolymer is 5:100:1;
[0073] (3) The terpolymer is prepared into a solution with a concentration of 70 mg / L, and then compounded with polyepoxysuccinic acid with a concentration of 30 mg / L, wherein the molar ratio of the terpolymer to the polyepoxysuccinic acid is 2.3:1, to obtain the silica scale inhibitor of the present invention, calculated as JC-600-6.
[0074] Comparative Example 1
[0075] This comparative example was carried out according to the method of Example 1, except that step (3) was not performed, and the prepared silica scale inhibitor was designated as D-JC-600-1.
[0076] Comparative Example 2
[0077] This comparative example was carried out according to the method of Example 2, except that N-tert-butyl acrylamide was not added in step (1), and the prepared silica scale inhibitor was designated as D-JC-600-2.
[0078] Comparative Example 3
[0079] This comparative example was carried out according to the method of Example 2, except that polyethylene glycol was not added in step (1), and the prepared silica scale inhibitor was designated as D-JC-600-3.
[0080] Test Example 1
[0081] Experiment on the performance of CaSiO3 scale inhibition: First, a silicon solution is prepared with sodium silicate so that the mass concentration of silicon element is about 480 mg / L (in terms of SiO2). Nine polyethylene plastic bottles are numbered 1-10 in sequence, and 100 mL of the silicon solution is respectively transferred to 10 polyethylene plastic bottles. Then, the silicon scale inhibitor prepared in Examples 1-6 and Comparative Examples 1-3 is respectively added to the polyethylene plastic bottles 1-10 so that the effective concentration of the silicon scale inhibitor in the bottle is 100 mg / L. The polyethylene plastic bottle 10 is a blank sample. HCl and NaOH solutions are added to the polyethylene plastic bottles 1-10 to adjust the pH value of the solution to 7.5, and then a CaCl2 solution with a mass fraction of 10% (in terms of CaCO3) is added thereto so that the mass concentration of calcium ions in the solution is 500 mg / L. Then, the pH value of each solution in the polyethylene plastic bottles 1-10 was adjusted to 7.0±0.1 with HCl and NaOH, and the polyethylene plastic bottles 1-10 were placed in a 40°C constant temperature water bath, and 15 mL of the sample supernatant was taken every 12 hours within 48 hours, and filtered through a 0.45 um filter membrane. After diluting a certain multiple, a quantitative volume filter sample was taken, and the content of dissolved silicon in the solution was determined by molybdenum blue colorimetry, and the scale inhibition rate was calculated according to the following formula. The experimental results are shown in Table 1.
[0082]
[0083] Where:
[0084] C2——the dissolved silicon content in the solution of the polyethylene plastic bottles 1-9 after heating for 48 hours, mg / L;
[0085] C0——the dissolved silicon content in the solution of the polyethylene plastic bottle 10 after heating for 48 hours, mg / L;
[0086] C1——the dissolved silicon content in the solution of the polyethylene plastic bottles 1-10 when not heated, mg / L.
[0087] Table 1
[0088]
[0089]
[0090] Test Example 2
[0091] Experiment on the performance of preventing colloidal silica scale: This test example was tested according to the method described in Test Example 1, except that the polyethylene plastic bottles were numbered ⅰ-ⅸ in sequence, and no 10% by mass CaCl2 solution was added. The content of dissolved silicon in the polyethylene plastic bottle solutions ⅰ-ⅸ was determined by the standard test method, and the scale inhibition rate was calculated according to the following formula. The experimental results are shown in Table 1.
[0092]
[0093] Where:
[0094] C2——the dissolved silicon content in the solution of the polyethylene plastic bottles i-ix after heating for 48 hours, mg / L;
[0095] C0——the dissolved silicon content in the solution of the polyethylene plastic bottle x after heating for 48 hours, mg / L;
[0096] C1——the dissolved silicon content in the solution of the polyethylene plastic bottles ⅰ-ⅹ when not heated, mg / L.
[0097]
[0098]
[0099] It can be seen from the results of Table 1 and Table 2 that after heating for 48 hours, the remaining dissolved silicon mass concentration in the solution of the polyethylene plastic bottle 1-6 is relatively high, which is mainly attributed to the negatively charged dispersibility of silicon scale by the sulfonic acid group and the hydroxyl group in the terpolymer in the silicon scale inhibitor JC-600-1 to JC-600-6 prepared in Examples 1-6, which makes it have a better scale inhibition effect than the silicon scale inhibitor D-JC-600-2 and D-JC-600-3 prepared in Comparative Examples 8 and 9. At the same time, due to the compounding of polyepoxysuccinic acid, the calcium silicate scale inhibition ability of the silicon scale inhibitor JC-600-1 to JC-600-6 prepared in Examples 1-6 is further improved compared with Comparative Example 7. In addition, most of the silicon element in colloidal silica scale exists in the form of condensed silica and its polymer, which is more difficult to disperse. Therefore, the effect of the scale inhibitor in inhibiting colloidal silica scale is not as good as the performance of inhibiting CaSiO3 scale.
[0100] The preferred embodiments of the present invention are described in detail above, but the present invention is not limited thereto. Within the technical concept of the present invention, the technical solution of the present invention can be subjected to a variety of simple modifications, including the combination of various technical features in any other suitable manner, and these simple modifications and combinations should also be regarded as the contents disclosed by the present invention and belong to the protection scope of the present invention.
Claims
1. A silicon scale inhibitor, characterized in that: The silicon scale inhibitor contains a terpolymer and polyepoxysuccinic acid, wherein the terpolymer comprises a first structural unit, a second structural unit and a third structural unit, the first structural unit is provided by polyethylene glycol, the second structural unit is provided by N-tert-butyl acrylamide, and the third structural unit is provided by an acrylic acid-2-acrylamide-2-methylpropane sulfonic acid copolymer.
2. The silicon scale inhibitor according to claim 1, characterized in that: The weight average molecular weight of the terpolymer is 500-20,000, preferably 800-20,000.
3. The silicon scale inhibitor according to claim 1 or 2, characterized in that: In the terpolymer, the molar ratio of the first structural unit, the second structural unit and the third structural unit is (1-20): (20-200): 1, preferably (1-10): (20-150): 1; Preferably, the weight average molecular weight of the polyethylene glycol is 200-1500, more preferably 400-1200; Preferably, the weight average molecular weight of the acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer is 800-2000, preferably 1000-2000.
4. The silicon scale inhibitor according to any one of claims 1 to 3, characterized in that: The weight ratio of the terpolymer to the polyepoxysuccinic acid is 1-10:1, preferably 1-5:
1.
5. The silicon scale inhibitor according to claim 1 or 4, characterized in that: The weight average molecular weight of the polyepoxysuccinic acid is 400-1500, preferably 500-1500.
6. A method for preparing a silicon scale inhibitor, characterized in that: The method comprises the following steps: (1) in the presence of an initiator and liquid alkali, polymerizing polyethylene glycol and N-tert-butylacrylamide; (2) subjecting the reaction product of step (1) to a polymerization reaction with an acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer; (3) Mixing the reaction product of step (2) with polyepoxysuccinic acid.
7. The method according to claim 6, characterized in that The molar ratio of the polyethylene glycol, the N-tert-butylacrylamide and the copolymer of 2-acrylamide-2-methylpropanesulfonic acid is (1-20):(20-200):1, preferably (1-10):(20-150):
1.
8. The method according to claim 6 or 7, characterized in that: In step (1), the polymerization reaction conditions include: temperature of 50-150° C., time of 2-8 h, and pH of 8-11; Preferably, the weight average molecular weight of the polyethylene glycol is 200-1500, more preferably 500-1200. Preferably, the initiator is selected from at least one of ammonium persulfate, ammonium persulfate-sodium bisulfite and sodium bisulfite.
9. The method according to claim 6 or 7, characterized in that: In step (2), the polymerization reaction conditions include: temperature of 20-100° C. and time of 0.5-6 h; Preferably, the weight average molecular weight of the acrylic acid-2-acrylamide-2-methylpropanesulfonic acid copolymer is 800-2000, more preferably 1000-1800.
10. The method according to claim 6 or 7, characterized in that: In step (3), the weight ratio of the terpolymer to the polyepoxysuccinic acid is 1-10:1, preferably 1-5:1.
Citation Information
Patent Citations
Composite multi-component scale inhibitor for treating oil-field water and preparation thereof
CN101412567A
Preparation method and application of water-based polyacrylamide composite dispersion liquid
CN101845115A
Silica scale inhibitor, preparation method and application
CN109438610A
Composite scale inhibitor for circulating cooling water and preparation method thereof
CN109835989A
Phosphorus-free scale inhibitor for inhibiting silicon scale and preparation method of phosphorus-free scale inhibitor
CN113912195A
Cited By
High-efficiency environment-friendly scale inhibitor and preparation method thereof
CN122809657A