Concrete low-carbon glue reducing agent and preparation method thereof

Through the synergistic effect of glycerol, composite microcapsules and other components, the existing concrete glue reducing agent has solved the problems of high cement type requirements and complex production process, and achieved the effect of reducing cement usage and increasing concrete strength, which has improved the construction industry Application potential.

CN119080427AInactive Publication Date: 2024-12-06南通盛茂建材科技有限公司
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411334371.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-24
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The existing concrete glue reducing agent has high requirements for cement types, limited applicability, complex production processes and high costs, resulting in limited application in the construction industry.

Method used

The synergistic efficiency mechanism of glycerol, composite microcapsules, mixed powder, cellulose ether, sodium thiosulfate and emulsified dispersant is adopted to reduce the amount of cement used to improve the flowability and hydration reaction of cement slurry and increase the concrete. Strength and wear resistance.

Benefits of technology

It has achieved significant reduction in cement usage while ensuring the strength of concrete, improved the density and durability of concrete, reduced production costs, and improved construction efficiency.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of concrete additives, and particularly provides a concrete low-carbon glue reducing agent and a preparation method thereof. The glue reducing agent is prepared by the following method: firstly, mixing 20-45 parts of glycerol, 3-6 parts of mixed powder and 55-70 parts of deionized water, and performing ultrasonic dispersion to obtain a mixed solution; then adding 5-8 parts of cellulose ether and 3-6 parts of sodium thiosulfate into the mixed solution, heating and uniformly stirring, then adding 10-20 parts of composite microcapsules, ultrasonically dispersing, heating, dropwise adding 0.5-1.0 part of emulsifying dispersant while stirring, keeping the temperature for 1-3 hours, and then cooling to obtain the glue reducing agent. The cement reducing agent disclosed by the invention is simple in preparation process, cement particles are fully dispersed and prevented from being agglomerated under the action of the glycerol and the mixed powder in the cement reducing agent under the action of the composite microcapsules, so that the use amount of cement in concrete with the same strength grade is greatly reduced, the workability of the concrete is improved, and the strength of the concrete is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of concrete additives, and in particular to a concrete low-carbon adhesive reducer and a preparation method thereof. Background Art

[0002] Concrete is an artificial stone made of cement as the main cementitious material, mixed with water, sand, gravel, and a certain amount of chemical admixtures and mineral admixtures when necessary, in an appropriate proportion, and then mixed evenly, compacted, formed, and cured. However, the cement production process is accompanied by high energy consumption, increased environmental pollution, and significant carbon emissions, which poses a severe challenge to the environment.

[0003] Concrete glue reducer is a new type of concrete admixture different from concrete water reducer. Glue reducer is also called concrete synergist or concrete fortifier. Its main function is to improve the workability of concrete, increase the overall glue content of concrete, and promote the hydration reaction of cement to be more complete, so as to reduce the amount of cement or other cementitious materials, thereby reducing the surface cracks of concrete caused by the heat of cement hydration. Glue reducer has high requirements for materials, especially the lack of sufficient flexibility in the selection of cement types. Different types and grades of cement have different mineral compositions and physical and chemical properties, which limits the applicability of glue reducer in different cements. Secondly, under the premise of ensuring the strength of concrete, the effect of existing glue reducer in reducing cement dosage is limited, generally only between 5% and 10%. However, in actual applications, as the amount of cement is reduced, other cementitious materials or admixtures are often needed to compensate for the loss of strength, thereby increasing costs. Furthermore, the production process of glue reducer is relatively complicated, and the cost of raw materials required is relatively high. This not only increases the production cost, but also indirectly pushes up the market price of glue reducer, limiting its wide application in the construction industry. The combined effect of these factors has resulted in certain restrictions on the practical application of glue reducers.

[0004] Based on the above statements, the present invention provides a low-carbon concrete adhesive reducer and a preparation method thereof. Summary of the invention

[0005] In order to solve the problems in the prior art that concrete glue reducers have high requirements on materials, cement reduction is not as expected, and the production process is complicated, the present invention provides a concrete low-carbon glue reducer and a preparation method thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions: A low-carbon concrete glue reducing agent comprises the following raw materials in parts by weight: 20-45 parts of glycerol, 10-20 parts of composite microcapsules, 3-6 parts of mixed powder, 5-8 parts of cellulose ether, 3-6 parts of sodium thiosulfate, 0.5-1.0 parts of emulsifying dispersant and 55-70 parts of deionized water.

[0007] Preferably, the composite microcapsule is prepared by the following method: (1) Mixing urea-formaldehyde resin and ethanol solution in a mass ratio of 1:8-12 and stirring for 10-20 minutes to obtain a urea-formaldehyde resin solution, adding 3-5% of polyethylene glycol fatty acid ester by mass of the urea-formaldehyde resin solution, and dispersing at 40-60°C and 80-100kHz for 10-15 minutes to obtain an emulsified solution A; (2) Mixing a polyurethane and a dichloromethane solution in a mass ratio of 1:8-12, dispersing at 80-100 kHz for 10-15 minutes to obtain a polyurethane solution, adding poloxamer in an amount of 3-6% by mass of the polyurethane solution, and stirring at room temperature for 10-15 minutes to obtain an emulsified solution B; (3) Emulsified solution A and emulsified solution B are mixed to obtain a mixed emulsified solution, an auxiliary agent is added to the mixed emulsified solution, the mixture is stirred for 10-15 minutes, and then centrifuged and dried to obtain composite microcapsules.

[0008] Preferably, the auxiliary agent in step (3) comprises 4,4'-diaminodiphenyl ether and 5-isocyanate isopeptide chloride in a mass ratio of 1:1-3.

[0009] Preferably, in step (3), the mass ratio of the emulsified solution A to the emulsified solution B is 1:1.5-2.5; and the mass ratio of the mixed emulsified solution to the auxiliary agent is 100:2-5.

[0010] Preferably, the centrifugal drying in step (3) is specifically: centrifuging at a rotation speed of 8000-10000 rpm for 5-8 min, filtering, and vacuum drying at 50-70° C. for 3-5 h.

[0011] Preferably, the mixed powder comprises nano-hydroxyapatite, nano-alumina and activated fly ash in a mass ratio of 1:0.3-0.5:0.5-0.8.

[0012] Preferably, the activated fly ash is prepared by the following method: stirring fly ash and mixed salt solution in a mass ratio of 1:8-12 at 40-60°C for 10-25 minutes, filtering, and drying at 80-100°C to obtain activated fly ash.

[0013] Preferably, the mixed salt solution comprises a sodium sulfate solution with a mass fraction of 20% and a calcium chloride solution with a mass fraction of 30% in a mass ratio of 1:1.

[0014] Preferably, the emulsifying dispersant includes one or more of polyethylene glycol monooleate, sodium lauryl sulfate, sodium cellulose sulfonate, and sodium pyrophosphate.

[0015] A method for preparing a low-carbon concrete adhesive reducing agent comprises the following steps: S1, mixing the glycerol, mixed powder and deionized water in the above-mentioned mass parts, dispersing at 150-200kHz for 10-15min, and then stirring at 40-60°C for 15-25min to obtain a mixed solution; S2. Add cellulose ether and sodium thiosulfate to the mixed solution, stir at 40-60° C. for 25-40 min; then add the composite microcapsule, disperse at 150-200 kHz for 10-15 min, add the emulsifying dispersant while stirring at 40-60° C., continue heating and stirring for 1-3 h after the addition is completed, and obtain the gelling agent after cooling.

[0016] In summary, the present invention has the following beneficial effects: The components of the low-carbon concrete gel reducer provided by the present invention integrate the synergistic mechanism of glycerol, composite microcapsules and mixed powder. This combination not only ensures the strength of concrete but also reduces the amount of cement. By introducing cellulose ether, the ether bonds on the molecules form hydrogen bonds with water molecules, which improves the fluidity of cement paste, thereby reducing the resistance between cement particles and accelerating the hydration of cement.

[0017] Introducing nano-hydroxyapatite, nano-alumina and activated fly ash into the glue reducer can significantly improve the strength and wear resistance of the glue reducer itself, which can help the glue reducer to better resist wear during use and extend its service life; nano-alumina helps to improve the flow properties of the glue reducer, thereby improving construction efficiency during use; activated fly ash promotes the formation of concrete structure and enhances the strength and durability of concrete through its unique hydration effect.

[0018] The low-carbon concrete gel reducer of the present invention improves the uniformity of dispersion of cement particles and fine aggregates in the mixed system by adjusting the energy balance of the solid-liquid interface in the mixture. This improvement not only effectively disperses cement molecules, reduces the ineffective flocculation and aggregation of powder materials, but also promotes full contact and reaction between cement particles. As the hydration reaction proceeds more fully, the density and durability of concrete are fundamentally improved. DETAILED DESCRIPTION

[0019] In order to make the implementation methods of the present application easier to understand, the present application will be described in detail below in conjunction with specific examples. These examples are only for illustration and are not limited to the scope of application of the present application.

[0020] Example 1 A low-carbon concrete glue reducing agent comprises the following raw materials in parts by weight: 20 parts of glycerol, 10 parts of composite microcapsules, 3 parts of mixed powder, 5 parts of cellulose ether, 3 parts of sodium thiosulfate, 0.5 parts of polyethylene glycol monooleate, and 55 parts of deionized water.

[0021] The composite microcapsules are prepared by the following method: (1) A urea-formaldehyde resin with a mass ratio of 1:8 and an ethanol solution with a mass fraction of 50% were mixed and stirred at 200 rpm for 10 min to obtain a urea-formaldehyde resin solution, and then a polyethylene glycol fatty acid ester with a mass fraction of 3% of the urea-formaldehyde resin solution was added, and the mixture was dispersed at 40°C and 80 kHz for 15 min to obtain an emulsified solution A; (2) polyurethane with a mass ratio of 1:8 and a dichloromethane solution with a mass fraction of 30% were mixed, dispersed at 100 kHz for 10 minutes to obtain a polyurethane solution, and then poloxamer with a mass fraction of 3% of the polyurethane solution was added, and stirred at room temperature at a speed of 200 rpm for 15 minutes to obtain an emulsified solution B; (3) Emulsified solution A and emulsified solution B with a mass ratio of 1:1.5 were stirred at 200 rpm for 10 min to obtain a mixed emulsified solution, and an auxiliary agent was added to the mixed emulsified solution. The mass ratio of the mixed emulsified solution to the auxiliary agent was 100:2. After stirring at 200 rpm for 15 min, the mixture was centrifuged at a speed of 8000 rpm for 8 min, filtered, and vacuum dried at 50°C for 5 h to obtain composite microcapsules.

[0022] The auxiliary agent comprises 4,4'-diaminodiphenyl ether and 5-isocyanate isopeptide chloride in a mass ratio of 1:1.

[0023] The mixed powder is nano-hydroxyapatite, nano-alumina and activated fly ash in a ratio of 1:0.3:0.5; the activated fly ash is prepared by the following method: fly ash and mixed salt solution in a mass ratio of 1:8 are stirred at 40°C for 25 minutes, filtered, and dried at 100°C to obtain the activated fly ash. The particle size of the activated fly ash is controlled at 100 μm.

[0024] The mixed salt solution includes a sodium sulfate solution with a mass fraction of 20% and a calcium chloride solution with a mass fraction of 30% in a mass ratio of 1:1.

[0025] A method for preparing a low-carbon concrete adhesive reducing agent comprises the following steps: S1, mixing the glycerol, mixed powder and deionized water in the above-mentioned mass parts, dispersing at 150 kHz for 15 minutes, and then stirring at 40° C. and 200 rpm for 25 minutes to obtain a mixed solution; S2, adding cellulose ether and sodium thiosulfate to the mixed solution, stirring at 40°C for 40 minutes; adding composite microcapsules, dispersing at 150kHz for 15 minutes, adding polyethylene glycol monooleate while stirring at 60°C, and after the addition is completed, continuing heating and stirring for 1 hour, and cooling to obtain a gel reducer. The stirring rate is controlled at 200rpm.

[0026] Example 2 A low-carbon concrete glue reducing agent comprises the following raw materials in parts by weight: 45 parts of glycerin, 20 parts of composite microcapsules, 6 parts of mixed powder, 8 parts of cellulose ether, 6 parts of sodium thiosulfate, 1.0 part of sodium lauryl sulfate, and 70 parts of deionized water.

[0027] The composite microcapsules are prepared by the following method: (1) A urea-formaldehyde resin with a mass ratio of 1:12 and an ethanol solution with a mass fraction of 50% were mixed and stirred at 220 rpm for 20 min to obtain a urea-formaldehyde resin solution, and then a polyethylene glycol fatty acid ester with a mass fraction of 5% of the urea-formaldehyde resin solution was added, and the mixture was dispersed at 60°C and 100 kHz for 10 min to obtain an emulsified solution A; (2) polyurethane with a mass ratio of 1:12 and a dichloromethane solution with a mass fraction of 30% were mixed, dispersed at 80 kHz for 15 minutes to obtain a polyurethane solution, and then poloxamer with a mass fraction of 6% of the polyurethane solution was added, and stirred at room temperature at a speed of 220 rpm for 10 minutes to obtain an emulsified solution B; (3) Emulsified solution A and emulsified solution B with a mass ratio of 1:2.5 were stirred at 220 rpm for 8 min to obtain a mixed emulsified solution, and an auxiliary agent was added to the mixed emulsified solution. The mass ratio of the mixed emulsified solution to the auxiliary agent was 100:5. After mixing and stirring at 220 rpm for 10 min, the mixture was centrifuged at a speed of 10000 rpm for 5 min, filtered, and vacuum dried at 70°C for 3 h to obtain composite microcapsules.

[0028] The auxiliary agent comprises 4,4'-diaminodiphenyl ether and 5-isocyanate isopeptide chloride in a mass ratio of 1:3.

[0029] The mixed powder is nano-hydroxyapatite, nano-alumina and activated fly ash in a ratio of 1:0.5:0.8; the activated fly ash is prepared by the following method: fly ash and mixed salt solution in a mass ratio of 1:12 are stirred at 60°C for 10 minutes, filtered, and dried at 80°C to obtain the activated fly ash. The particle size of the activated fly ash is controlled at 100 μm.

[0030] The mixed salt solution includes a sodium sulfate solution with a mass fraction of 20% and a calcium chloride solution with a mass fraction of 30% in a mass ratio of 1:1.

[0031] A method for preparing a low-carbon concrete adhesive reducing agent comprises the following steps: S1, mixing the glycerol, mixed powder and deionized water in the above-mentioned mass parts, dispersing at 200 kHz for 10 min, and then stirring at 60° C. and 150 rpm for 15 min to obtain a mixed solution; S2, adding cellulose ether and sodium thiosulfate to the mixed solution, stirring at 60°C for 25 minutes; adding composite microcapsules, dispersing at 200kHz for 10 minutes, adding sodium lauryl sulfate at 40°C while stirring, and after the addition is completed, continuing heating and stirring for 3 hours, and cooling to obtain a gelling agent. The stirring rate is controlled at 150rpm.

[0032] Example 3 A low-carbon concrete glue reducing agent comprises the following raw materials in parts by weight: 30 parts of glycerin, 15 parts of composite microcapsules, 5 parts of mixed powder, 7 parts of cellulose ether, 5 parts of sodium thiosulfate, 0.8 parts of sodium lauryl sulfate, and 65 parts of deionized water.

[0033] The composite microcapsules are prepared by the following method: (1) A urea-formaldehyde resin with a mass ratio of 1:10 and an ethanol solution with a mass fraction of 50% were mixed and stirred at 300 rpm for 15 min to obtain a urea-formaldehyde resin solution, and then a polyethylene glycol fatty acid ester with a mass fraction of 4% of the urea-formaldehyde resin solution was added, and the mixture was dispersed at 50°C and 90 kHz for 12 min to obtain an emulsified solution A; (2) polyurethane with a mass ratio of 1:10 and a dichloromethane solution with a mass fraction of 30% were mixed, dispersed at 100 kHz for 13 minutes to obtain a polyurethane solution, and then poloxamer with a mass fraction of 5% of the polyurethane solution was added, and stirred at room temperature at a speed of 240 rpm for 12 minutes to obtain an emulsified solution B; (3) Emulsified solution A and emulsified solution B with a mass ratio of 1:2.0 were stirred at 240 rpm for 10 min to obtain a mixed emulsified solution, and an auxiliary agent was added to the mixed emulsified solution. The mass ratio of the mixed emulsified solution to the auxiliary agent was 100:3. After mixing and stirring at 240 rpm for 12 min, the mixture was centrifuged at a speed of 9000 rpm for 7 min, filtered, and vacuum dried at 60°C for 4 h to obtain composite microcapsules.

[0034] The auxiliary agent comprises 4,4'-diaminodiphenyl ether and 5-isocyanate isopeptide chloride in a mass ratio of 1:2.

[0035] The mixed powder is nano-hydroxyapatite, nano-alumina and activated fly ash in a ratio of 1:0.4:0.7; the activated fly ash is prepared by the following method: fly ash and mixed salt solution in a mass ratio of 1:10 are stirred at 50°C for 18 minutes, filtered, and dried at 90°C to obtain the activated fly ash. The particle size of the activated fly ash is controlled at 100 μm.

[0036] The mixed salt solution includes a sodium sulfate solution with a mass fraction of 20% and a calcium chloride solution with a mass fraction of 30% in a mass ratio of 1:1.

[0037] A method for preparing a low-carbon concrete adhesive reducing agent comprises the following steps: S1, mixing the glycerol, mixed powder and deionized water in the mass parts, dispersing at 180 kHz for 12 min, and then stirring at 50° C. and 180 rpm for 20 min to obtain a mixed solution; S2, adding cellulose ether and sodium thiosulfate to the mixed solution, stirring at 50°C for 35 minutes; adding composite microcapsules, dispersing at 180kHz for 13 minutes, adding sodium pyrophosphate while stirring at 50°C, and after the addition is completed, continuing heating and stirring for 2 hours, and cooling to obtain a gelling agent. The stirring rate is controlled at 180rpm.

[0038] Example 4 A low-carbon concrete glue reducing agent comprises the following raw materials in parts by weight: 35 parts of glycerol, 10 parts of composite microcapsules, 4 parts of mixed powder, 6 parts of cellulose ether, 5 parts of sodium thiosulfate, 0.8 parts of sodium lauryl sulfate, and 65 parts of deionized water.

[0039] The composite microcapsules are prepared by the following method: (1) A urea-formaldehyde resin with a mass ratio of 1:9 and an ethanol solution with a mass fraction of 50% were mixed and stirred at 250 rpm for 18 minutes to obtain a urea-formaldehyde resin solution, and then a polyethylene glycol fatty acid ester with a mass fraction of 3% of the urea-formaldehyde resin solution was added, and the mixture was dispersed at 45°C and 100 kHz for 15 minutes to obtain an emulsified solution A; (2) polyurethane with a mass ratio of 1:10 and a dichloromethane solution with a mass fraction of 30% were mixed, dispersed at 100 kHz for 10 minutes to obtain a polyurethane solution, and then poloxamer with a mass fraction of 5% of the polyurethane solution was added, and stirred at room temperature at a speed of 250 rpm for 13 minutes to obtain an emulsified solution B; (3) Emulsified solution A and emulsified solution B in a mass ratio of 1:2.5 were stirred at 250 rpm for 8 min to obtain a mixed emulsified solution, and an auxiliary agent was added to the mixed emulsified solution. The mass ratio of the mixed emulsified solution to the auxiliary agent was 100:4. After mixing and stirring at a speed of 240 rpm for 14 min, the mixture was centrifuged at a speed of 9000 rpm for 8 min, filtered, and vacuum dried at 55 °C for 3.5 h to obtain composite microcapsules.

[0040] The auxiliary agent comprises 4,4'-diaminodiphenyl ether and 5-isocyanate isopeptide chloride in a mass ratio of 1:1.

[0041] The mixed powder is nano-hydroxyapatite, nano-alumina and activated fly ash in a ratio of 1:0.5:0.5; the activated fly ash is prepared by the following method: fly ash and mixed salt solution in a mass ratio of 1:9 are stirred at 55°C for 18 minutes, filtered, and dried at 100°C to obtain the activated fly ash. The particle size of the activated fly ash is controlled at 100 μm.

[0042] The mixed salt solution includes a sodium sulfate solution with a mass fraction of 20% and a calcium chloride solution with a mass fraction of 30% in a mass ratio of 1:1.

[0043] A method for preparing a low-carbon concrete adhesive reducing agent comprises the following steps: S1, mixing the glycerol, mixed powder and deionized water in the mass parts, dispersing at 150 kHz for 14 min, and then stirring at 45° C. and 180 rpm for 18 min to obtain a mixed solution; S2, adding cellulose ether and sodium thiosulfate to the mixed solution, stirring at 55°C for 35 minutes; adding composite microcapsules, dispersing at 200kHz for 14 minutes, adding sodium cellulose sulfonate at 45°C while stirring, and after the addition is completed, continuing heating and stirring for 2.5 hours, and cooling to obtain a gelling agent. The stirring rate is controlled at 180rpm.

[0044] Comparative Example 1 A low-carbon concrete glue reducing agent comprises the following raw materials in parts by weight: 35 parts of glycerol, 10 parts of composite microcapsules, 4 parts of mixed powder, 6 parts of cellulose ether, 5 parts of sodium thiosulfate, 0.8 parts of sodium lauryl sulfate, and 65 parts of deionized water.

[0045] The composite microcapsules are prepared by the following method: (1) Urea-formaldehyde resin, polyurethane and 50% ethanol solution in a mass ratio of 1:1:9 were mixed and stirred at 250 rpm for 18 min to obtain a urea-formaldehyde resin solution, and then polyethylene glycol fatty acid ester in an amount of 3% by mass of the urea-formaldehyde resin solution was added, and the mixture was dispersed at 45°C and 100 kHz for 15 min to obtain an emulsified solution; (2) Adding an auxiliary agent to the emulsified solution at a mass ratio of 100:4, stirring at 240 rpm for 14 min, centrifuging at 9000 rpm for 8 min, filtering, and vacuum drying at 55 °C for 3.5 h to obtain composite microcapsules.

[0046] The auxiliary agent comprises 4,4'-diaminodiphenyl ether and 5-isocyanate isopeptide chloride in a mass ratio of 1:1.

[0047] The mixed powder is nano-hydroxyapatite, nano-alumina and activated fly ash in a ratio of 1:0.5:0.5; the activated fly ash is prepared by the following method: fly ash and mixed salt solution in a mass ratio of 1:9 are stirred at 55°C for 18 minutes, filtered, and dried at 100°C to obtain the activated fly ash. The particle size of the activated fly ash is controlled at 100 μm.

[0048] The mixed salt solution includes a sodium sulfate solution with a mass fraction of 20% and a calcium chloride solution with a mass fraction of 30% in a mass ratio of 1:1.

[0049] A method for preparing a low-carbon concrete adhesive reducing agent comprises the following steps: S1, mixing the glycerol, mixed powder and deionized water in the mass parts, dispersing at 150 kHz for 14 min, and then stirring at 45° C. and 180 rpm for 18 min to obtain a mixed solution; S2, adding cellulose ether and sodium thiosulfate to the mixed solution, stirring at 55°C for 35 minutes; adding composite microcapsules, dispersing at 200kHz for 14 minutes, adding sodium cellulose sulfonate at 45°C while stirring, and after the addition is completed, continuing heating and stirring for 2.5 hours, and cooling to obtain a gelling agent. The stirring rate is controlled at 180rpm.

[0050] Comparative Example 2 A low-carbon concrete glue reducing agent comprises the following raw materials in parts by weight: 35 parts of glycerol, 10 parts of composite microcapsules, 4 parts of mixed powder, 6 parts of cellulose ether, 5 parts of sodium thiosulfate, 0.8 parts of sodium lauryl sulfate, and 65 parts of deionized water.

[0051] The composite microcapsules are prepared by the following method: (1) A urea-formaldehyde resin with a mass ratio of 1:9 and an ethanol solution with a mass fraction of 50% were mixed and stirred at 250 rpm for 18 minutes to obtain a urea-formaldehyde resin solution, and then a polyethylene glycol fatty acid ester with a mass fraction of 3% of the urea-formaldehyde resin solution was added, and the mixture was dispersed at 45°C and 100 kHz for 15 minutes to obtain an emulsified solution A; (2) polyurethane with a mass ratio of 1:10 and a dichloromethane solution with a mass fraction of 30% were mixed, dispersed at 100 kHz for 10 minutes to obtain a polyurethane solution, and then poloxamer with a mass fraction of 5% of the polyurethane solution was added, and stirred at room temperature at a speed of 250 rpm for 13 minutes to obtain an emulsified solution B; (3) Emulsified solution A and emulsified solution B in a mass ratio of 1:2.5 were stirred at 250 rpm for 8 min to obtain a mixed emulsified solution, and an auxiliary agent was added to the mixed emulsified solution. The mass ratio of the mixed emulsified solution to the auxiliary agent was 100:4. After mixing and stirring at a speed of 240 rpm for 14 min, the mixture was centrifuged at a speed of 9000 rpm for 8 min, filtered, and vacuum dried at 55 °C for 3.5 h to obtain composite microcapsules.

[0052] The auxiliary agent comprises 4,4'-diaminodiphenyl ether and 5-isocyanate isopeptide chloride in a mass ratio of 1:1.

[0053] The mixed powder is nano hydroxyapatite, nano alumina and fly ash in a ratio of 1:0.5:0.5.

[0054] The mixed salt solution includes a sodium sulfate solution with a mass fraction of 20% and a calcium chloride solution with a mass fraction of 30% in a mass ratio of 1:1.

[0055] A method for preparing a low-carbon concrete adhesive reducing agent comprises the following steps: S1, mixing the glycerol, mixed powder and deionized water in the above-mentioned mass parts, dispersing at 150 kHz for 14 minutes, and then stirring at 45° C. for 18 minutes to obtain a mixed solution; S2, adding cellulose ether and sodium thiosulfate to the mixed solution, stirring at 55°C for 35 minutes; adding composite microcapsules, dispersing at 200kHz for 14 minutes, adding sodium cellulose sulfonate at 45°C while stirring, and after the addition is completed, continuing heating and stirring for 2.5 hours, and cooling to obtain a gelling agent. The stirring rate is controlled at 180rpm.

[0056] Comparative Example 3 A low-carbon concrete glue reducing agent comprises the following raw materials in parts by weight: 35 parts of glycerol, 10 parts of composite microcapsules, 4 parts of mixed powder, 6 parts of cellulose ether, 5 parts of sodium thiosulfate, 0.8 parts of sodium lauryl sulfate, and 65 parts of deionized water.

[0057] The composite microcapsules are prepared by the following method: (1) A urea-formaldehyde resin with a mass ratio of 1:9 and an ethanol solution with a mass fraction of 50% were mixed and stirred at 250 rpm for 18 minutes to obtain a urea-formaldehyde resin solution, and then a polyethylene glycol fatty acid ester with a mass fraction of 3% of the urea-formaldehyde resin solution was added, and the mixture was dispersed at 45°C and 100 kHz for 15 minutes to obtain an emulsified solution A; (2) polyurethane with a mass ratio of 1:10 and a dichloromethane solution with a mass fraction of 30% were mixed, dispersed at 100 kHz for 10 minutes to obtain a polyurethane solution, and then poloxamer with a mass fraction of 5% of the polyurethane solution was added, and stirred at room temperature at a speed of 250 rpm for 13 minutes to obtain an emulsified solution B; (3) Emulsified solution A and emulsified solution B in a mass ratio of 1:2.5 were stirred at 250 rpm for 8 min to obtain a mixed emulsified solution, and an auxiliary agent was added to the mixed emulsified solution. The mass ratio of the mixed emulsified solution to the auxiliary agent was 100:4. After mixing and stirring at a speed of 240 rpm for 14 min, the mixture was centrifuged at a speed of 9000 rpm for 8 min, filtered, and vacuum dried at 55 °C for 3.5 h to obtain composite microcapsules.

[0058] The auxiliary agent comprises 4,4'-diaminodiphenyl ether and 5-isocyanate isopeptide chloride in a mass ratio of 1:1.

[0059] The mixed powder is nano-alumina and activated fly ash in a ratio of 1.5:0.5; the activated fly ash is prepared by the following method: fly ash and mixed salt solution in a mass ratio of 1:9 are stirred at 55°C for 18 minutes, filtered, and dried at 100°C to obtain the activated fly ash. The particle size of the activated fly ash is controlled at 100 μm.

[0060] The mixed salt solution includes a sodium sulfate solution with a mass fraction of 20% and a calcium chloride solution with a mass fraction of 30% in a mass ratio of 1:1.

[0061] A method for preparing a low-carbon concrete adhesive reducing agent comprises the following steps: S1, mixing the glycerol, mixed powder and deionized water in the mass parts, dispersing at 150 kHz for 14 min, and then stirring at 45° C. and 180 rpm for 18 min to obtain a mixed solution; S2, adding cellulose ether and sodium thiosulfate to the mixed solution, stirring at 55°C for 35 minutes; adding composite microcapsules, dispersing at 200kHz for 14 minutes, adding sodium cellulose sulfonate at 45°C while stirring, and after the addition is completed, continuing heating and stirring for 2.5 hours, and cooling to obtain a gelling agent. The stirring rate is controlled at 180rpm.

[0062] Comparative Example 4 A low-carbon concrete glue reducing agent comprises the following raw materials in parts by weight: 35 parts of glycerol, 10 parts of composite microcapsules, 4 parts of mixed powder, 6 parts of cellulose ether, 5 parts of sodium thiosulfate, 0.8 parts of sodium lauryl sulfate, and 65 parts of deionized water.

[0063] The composite microcapsules are prepared by the following method: (1) A urea-formaldehyde resin with a mass ratio of 1:9 and an ethanol solution with a mass fraction of 50% were mixed and stirred at 250 rpm for 18 minutes to obtain a urea-formaldehyde resin solution, and then a polyethylene glycol fatty acid ester with a mass fraction of 3% of the urea-formaldehyde resin solution was added, and the mixture was dispersed at 45°C and 100 kHz for 15 minutes to obtain an emulsified solution A; (2) polyurethane with a mass ratio of 1:10 and a dichloromethane solution with a mass fraction of 30% were mixed, dispersed at 100 kHz for 10 minutes to obtain a polyurethane solution, and then poloxamer with a mass fraction of 5% of the polyurethane solution was added, and stirred at room temperature at a speed of 250 rpm for 13 minutes to obtain an emulsified solution B; (3) Emulsified solution A and emulsified solution B in a mass ratio of 1:2.5 were stirred at 250 rpm for 8 min to obtain a mixed emulsified solution, and an auxiliary agent was added to the mixed emulsified solution. The mass ratio of the mixed emulsified solution to the auxiliary agent was 100:4. After mixing and stirring at a speed of 240 rpm for 14 min, the mixture was centrifuged at a speed of 9000 rpm for 8 min, filtered, and vacuum dried at 55 °C for 3.5 h to obtain composite microcapsules.

[0064] The auxiliary agent comprises 4,4'-diaminodiphenyl ether and 5-isocyanate isopeptide chloride in a mass ratio of 1:1.

[0065] The mixed powder is nano-hydroxyapatite and activated fly ash in a ratio of 1.5:0.5; the activated fly ash is prepared by the following method: fly ash and mixed salt solution in a mass ratio of 1:9 are stirred at 55°C for 18 minutes, filtered, and dried at 100°C to obtain activated fly ash.

[0066] The mixed salt solution includes a sodium sulfate solution with a mass fraction of 20% and a calcium chloride solution with a mass fraction of 30% in a mass ratio of 1:1.

[0067] A method for preparing a low-carbon concrete adhesive reducing agent comprises the following steps: S1, mixing the glycerol, mixed powder and deionized water in the above-mentioned mass parts, dispersing at 150 kHz for 14 minutes, and then stirring at 45° C. for 18 minutes to obtain a mixed solution; S2, adding cellulose ether and sodium thiosulfate to the mixed solution, stirring at 55°C for 35 minutes; adding composite microcapsules, dispersing at 200kHz for 14 minutes, adding sodium cellulose sulfonate at 45°C while stirring, and after the addition is completed, continuing heating and stirring for 2.5 hours, and cooling to obtain a gelling agent. The stirring rate is controlled at 180rpm.

[0068] Comparative Example 5 A low-carbon concrete glue reducing agent comprises the following raw materials in parts by weight: 35 parts of glycerol, 10 parts of composite microcapsules, 4 parts of mixed powder, 6 parts of cellulose ether, 5 parts of sodium thiosulfate, 0.8 parts of sodium lauryl sulfate, and 65 parts of deionized water.

[0069] The composite microcapsules are prepared by the following method: (1) A urea-formaldehyde resin with a mass ratio of 1:9 and an ethanol solution with a mass fraction of 50% were mixed and stirred at 250 rpm for 18 minutes to obtain a urea-formaldehyde resin solution, and then a polyethylene glycol fatty acid ester with a mass fraction of 3% of the urea-formaldehyde resin solution was added, and the mixture was dispersed at 45°C and 100 kHz for 15 minutes to obtain an emulsified solution A; (2) polyurethane with a mass ratio of 1:10 and a dichloromethane solution with a mass fraction of 30% were mixed, dispersed at 100 kHz for 10 minutes to obtain a polyurethane solution, and then poloxamer with a mass fraction of 5% of the polyurethane solution was added, and stirred at room temperature at a speed of 250 rpm for 13 minutes to obtain an emulsified solution B; (3) Emulsified solution A and emulsified solution B in a mass ratio of 1:2.5 were stirred at 250 rpm for 8 min to obtain a mixed emulsified solution, and an auxiliary agent was added to the mixed emulsified solution. The mass ratio of the mixed emulsified solution to 4,4'-diaminodiphenyl ether was 100:4. After mixing and stirring at a speed of 240 rpm for 14 min, the mixture was centrifuged at a speed of 9000 rpm for 8 min, filtered, and vacuum dried at 55 °C for 3.5 h to obtain composite microcapsules.

[0070] The mixed powder is nano-hydroxyapatite, nano-alumina and activated fly ash in a ratio of 1:0.5:0.5; the activated fly ash is prepared by the following method: fly ash and mixed salt solution in a mass ratio of 1:9 are stirred at 55°C for 18 minutes, filtered, and dried at 100°C to obtain the activated fly ash. The particle size of the activated fly ash is controlled at 100 μm.

[0071] The mixed salt solution includes a sodium sulfate solution with a mass fraction of 20% and a calcium chloride solution with a mass fraction of 30% in a mass ratio of 1:1.

[0072] A method for preparing a low-carbon concrete adhesive reducing agent comprises the following steps: S1, mixing the glycerol, mixed powder and deionized water in the mass parts, dispersing at 150 kHz for 14 min, and then stirring at 45° C. and 180 rpm for 18 min to obtain a mixed solution; S2, adding cellulose ether and sodium thiosulfate to the mixed solution, stirring at 55°C for 35 minutes; adding composite microcapsules, dispersing at 200kHz for 14 minutes, adding sodium cellulose sulfonate at 45°C while stirring, and after the addition is completed, continuing heating and stirring for 2.5 hours, and cooling to obtain a gelling agent. The stirring rate is controlled at 180rpm.

[0073] Comparative Example 6 A low-carbon concrete glue reducing agent comprises the following raw materials in parts by weight: 35 parts of glycerol, 10 parts of composite microcapsules, 4 parts of mixed powder, 6 parts of cellulose ether, 5 parts of sodium thiosulfate, 0.8 parts of sodium lauryl sulfate, and 65 parts of deionized water.

[0074] The composite microcapsules are prepared by the following method: (1) A urea-formaldehyde resin with a mass ratio of 1:9 and an ethanol solution with a mass fraction of 50% were mixed and stirred at 250 rpm for 18 minutes to obtain a urea-formaldehyde resin solution, and then a polyethylene glycol fatty acid ester with a mass fraction of 3% of the urea-formaldehyde resin solution was added, and the mixture was dispersed at 45°C and 100 kHz for 15 minutes to obtain an emulsified solution A; (2) polyurethane with a mass ratio of 1:10 and a dichloromethane solution with a mass fraction of 30% were mixed, dispersed at 100 kHz for 10 minutes to obtain a polyurethane solution, and then poloxamer with a mass fraction of 5% of the polyurethane solution was added, and stirred at room temperature at a speed of 250 rpm for 13 minutes to obtain an emulsified solution B; (3) Emulsified solution A and emulsified solution B in a mass ratio of 1:2.5 were stirred at 250 rpm for 8 min to obtain a mixed emulsified solution, and an auxiliary agent was added to the mixed emulsified solution. The mass ratio of the mixed emulsified solution to 5-isocyanate isopeptide chloride was 100:4. After mixing and stirring at a speed of 240 rpm for 14 min, the mixture was centrifuged at a speed of 9000 rpm for 8 min, filtered, and vacuum dried at 55 °C for 3.5 h to obtain composite microcapsules.

[0075] The mixed powder is nano-hydroxyapatite, nano-alumina and activated fly ash in a ratio of 1:0.5:0.5; the activated fly ash is prepared by the following method: fly ash and mixed salt solution in a mass ratio of 1:9 are stirred at 55°C for 18 minutes, filtered, and dried at 100°C to obtain the activated fly ash. The particle size of the activated fly ash is controlled at 100 μm.

[0076] The mixed salt solution includes a sodium sulfate solution with a mass fraction of 20% and a calcium chloride solution with a mass fraction of 30% in a mass ratio of 1:1.

[0077] A method for preparing a low-carbon concrete adhesive reducing agent comprises the following steps: S1, mixing the glycerol, mixed powder and deionized water in the mass parts, dispersing at 150 kHz for 14 min, and then stirring at 45° C. and 180 rpm for 18 min to obtain a mixed solution; S2, adding cellulose ether and sodium thiosulfate to the mixed solution, stirring at 55°C for 35 minutes; adding composite microcapsules, dispersing at 200kHz for 14 minutes, adding sodium cellulose sulfonate at 45°C while stirring, and after the addition is completed, continuing heating and stirring for 2.5 hours, and cooling to obtain a gelling agent. The stirring rate is controlled at 180rpm.

[0078] Performance Testing The concrete adhesive reducer prepared in Examples 1-4 and Comparative Examples 1-6 of the present invention was applied to concrete and compared with a blank sample without adhesive reducer. Conch P042.5 cement was used, river sand (fineness modulus was 3.0) was used as the cement, and 5-30 mm continuous graded gravel was used as the gravel. The strength of the concrete was tested according to the test method specified in GB / T50081-2002. The workability of the concrete was tested according to the test method specified in GB / T50080-2016.

[0079] The blank concrete is a concrete mix without the addition of the adhesive reducing agent, and the test concrete is a concrete mix with the adhesive reducing agent of Examples 1-4 and Comparative Examples 1-6. The blank concrete and the test concrete mix are shown in Table 1, wherein the blank concrete is a concrete mix with the common commercial adhesive reducing agent.

[0080] Table 1 Concrete ingredients

[0081] Table 2 Concrete performance test results

[0082] From the results in Table 2, it can be seen that when the amount of concrete gel reducer prepared by the present invention is 0.8% of the mass of cement, the amount of cement in concrete can be reduced by 18%, while the 3d compressive strength of concrete is improved and the workability of concrete is excellent. According to the comparative example, the introduction of mixed powder can improve the performance of concrete while reducing the amount of cement. The introduction of composite microcapsules definitely helps to improve the strength of concrete. Through the synergistic effect between the components, the gelling particles are better dispersed, effectively promoting the hydration reaction efficiency of the system.

[0083] The above contents are merely examples and explanations of the present invention. Those skilled in the art may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the invention or exceed the scope defined by the claims, they shall all fall within the protection scope of the present invention.

Claims

1. A low-carbon concrete adhesive reducer, characterized in that: Including the following raw materials by weight: 20-45 parts of glycerol, 10-20 parts of composite microcapsules, 3-6 parts of mixed powder, 5-8 parts of cellulose ether, 3-6 parts of sodium thiosulfate, 0.5-1.0 parts of emulsifying dispersant, and 55-70 parts of deionized water.

2. A low-carbon concrete adhesive reducer according to claim 1, characterized in that: The composite microcapsules are prepared by the following method: (1) Mixing urea-formaldehyde resin and ethanol solution in a mass ratio of 1:8-12 and stirring for 10-20 minutes to obtain a urea-formaldehyde resin solution, adding 3-5% of polyethylene glycol fatty acid ester by mass of the urea-formaldehyde resin solution, and dispersing at 40-60°C and 80-100kHz for 10-15 minutes to obtain an emulsified solution A; (2) Mixing a polyurethane and a dichloromethane solution in a mass ratio of 1:8-12, dispersing at 80-100 kHz for 10-15 minutes to obtain a polyurethane solution, adding poloxamer in an amount of 3-6% by mass of the polyurethane solution, and stirring at room temperature for 10-15 minutes to obtain an emulsified solution B; (3) Emulsified solution A and emulsified solution B are mixed to obtain a mixed emulsified solution, an auxiliary agent is added to the mixed emulsified solution, the mixture is stirred for 10-15 minutes, and then centrifuged and dried to obtain composite microcapsules.

3. A low-carbon concrete adhesive reducer according to claim 2, characterized in that: The auxiliary agent in step (3) comprises 4,4'-diaminodiphenyl ether and 5-isocyanate isopeptide chloride in a mass ratio of 1:1-3.

4. A low-carbon concrete adhesive reducer according to claim 2, characterized in that: In the step (3), the mass ratio of the emulsified solution A to the emulsified solution B is 1:1.5-2.5; the mass ratio of the mixed emulsified solution to the auxiliary agent is 100:2-5.

5. A low carbon adhesive reducing agent for concrete according to claim 2, characterized in that: The centrifugal drying in step (3) is specifically as follows: centrifuging at a rotation speed of 8000-10000 rpm for 5-8 minutes, filtering, and vacuum drying at 50-70° C. for 3-5 hours.

6. A low carbon adhesive reducing agent for concrete according to claim 2, characterized in that: The mixed powder comprises nano hydroxyapatite, nano alumina and activated fly ash in a mass ratio of 1:0.3-0.5:0.5-0.

8.

7. A low carbon adhesive reducing agent for concrete according to claim 6, characterized in that: The activated fly ash is prepared by the following method: the fly ash and mixed salt solution with a mass ratio of 1:8-12 are stirred at 40-60°C for 10-25 minutes, filtered, and dried at 80-100°C to obtain the activated fly ash.

8. A low carbon adhesive reducing agent for concrete according to claim 7, characterized in that: The mixed salt solution includes a sodium sulfate solution with a mass fraction of 20% and a calcium chloride solution with a mass fraction of 30% in a mass ratio of 1:

1.

9. A low carbon adhesive reducing agent for concrete according to claim 1, characterized in that: The emulsifying dispersant includes one or more of polyethylene glycol monooleate, sodium lauryl sulfate, sodium cellulose sulfonate, and sodium pyrophosphate.

10. A method for preparing a low-carbon concrete adhesive reducer according to any one of claims 1 to 9, characterized in that: The following steps are involved: S1, mixing the glycerol, mixed powder and deionized water in the above-mentioned mass parts, dispersing at 150-200 kHz for 10-15 min, and stirring at 40-60° C. for 15-25 min to obtain a mixed solution; S2. Add cellulose ether and sodium thiosulfate to the mixed solution, stir at 40-60° C. for 25-40 min; then add the composite microcapsule, disperse at 150-200 kHz for 10-15 min, add the emulsifying dispersant while stirring at 40-60° C., continue heating and stirring for 1-3 h after the addition is completed, and obtain the gelling agent after cooling.