Modified phosphate-based inorganic polymer, and preparation method and application thereof

Through the combination of modifier and activated calcium oxide and metakaolin, the compressive strength and settling time of acid-excited inorganic polymers are improved, and the problems of slow curing and high shrinkage are solved, which are suitable for construction and environmental protection.

CN119080441APending Publication Date: 2024-12-06SOUTHWEAT UNIV OF SCI & TECH
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410951943.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-16
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The acid-excited inorganic polymer cures slowly at room temperature, has a long settling time, generates a lot of heat during stirring, and poor slurry flow performance, resulting in difficult construction, and high shrinkage affects practical application.

Method used

The mixed powder of modifier, activated calcium oxide and metakaolin is stirred with liquid raw materials of phosphoric acid, aluminum dihydrogen phosphate and water to form an inorganic polymer slurry, molded through molds and properly cured to control the settling time and shrinkage rate.

Benefits of technology

The compressive strength and dry shrinkage performance of the inorganic polymer are significantly improved, the settling time is controlled between 48 and 77 hours, the dry shrinkage rate is reduced, which is suitable for construction needs, and the environmental impact of the material is reduced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119080441A_ABST
    Figure CN119080441A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of inorganic cementing materials, and particularly relates to a modified phosphate-based inorganic polymer, a preparation method and application, the preparation method of the modified phosphate-based inorganic polymer comprises the following steps: S1, mixing and stirring a modifier, active calcium oxide and metakaolin to obtain a powder raw material, mixing phosphoric acid, aluminum dihydrogen phosphate and water to obtain a liquid raw material; mixing and stirring the powder raw material and the liquid raw material to obtain inorganic polymer slurry; and S2, pouring the inorganic polymer slurry obtained in the step S1 into a mold for molding to obtain a sample, and then curing the sample to obtain the modified phosphate-based inorganic polymer. The mechanical property of the modified phosphate-based inorganic polymer provided by the invention is remarkably improved, the utilization of the phosphate-based inorganic polymer can be realized, and the ecological environment can be improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of inorganic gelling materials, and in particular relates to a modified phosphoric acid-based inorganic polymer, a preparation method and an application thereof. Background Art

[0002] Inorganic polymers use aluminosilicate materials as precursors. Under the action of acidic or alkaline activators, the precursors dissolve and release aluminate and silicate monomers, which then undergo polycondensation reactions to form a gelling material composed of chain structural units such as -Si-O-Al-O-, -Si-O-Al-O-Si-O-, etc., with a three-dimensional network gel structure. In the internal structure of the three-dimensional network aluminosilicate gelling material, the silicon-oxygen tetrahedron structure can not only be interconnected with the aluminum-oxygen tetrahedron, but also with the combination of the silicon-oxygen tetrahedron structure and the aluminum-oxygen tetrahedron structure. This gelling material is also significantly different from the hydration product of ordinary silicate cement. After hydration, silicate cement mainly generates oligomers such as hydrated dicalcium silicate and hydrated tricalcium silicate, while the silicate-alumina gelling material mainly generates a network of inorganic polymers after polymerization. The polymerization reaction is different from the hydration reaction of calcium silicate. The final geopolymer is mainly composed of ionic bonds and covalent bonds, supplemented by van der Waals bonds and hydrogen bonds. Therefore, its performance is much better than that of traditional cement. In addition, most of the properties of silica-alumina cementitious materials are better than ordinary materials such as cement and ceramic polymers. This cementitious material has the excellent properties of polymers, ceramic materials and ordinary cement, and can combine the characteristics of the three. At the same time, its performance is better than any of the three materials. Compared with ordinary silicate cement, inorganic polymers not only have excellent mechanical strength and durability, but also reduce carbon emissions by 53%-72% during its production process, and have the characteristics of low carbon and environmental protection. In addition, on the one hand, the raw materials of inorganic polymers are widely available. Most of the industrial by-products of silicate sources, including mineral materials rich in silica-alumina materials such as kaolin, fly ash, slag, and construction material waste, can be used as raw materials for inorganic polymers; on the other hand, the preparation process of inorganic polymers does not require high-temperature calcination, so almost no NO is generated during the production process. x 、SO x Based on the above advantages, inorganic polymers are regarded as the most promising inorganic cementitious materials to replace ordinary Portland cement.

[0003] Acid-based inorganic polymers are formed by activating active silica-alumina raw materials with acid salts or inorganic acids. Active silica-alumina raw materials are mainly composed of metakaolin, fly ash and various industrial wastes. The categories of acid activators are mainly phosphoric acid and sulfuric acid and their acid salts. Compared with alkali-activated inorganic polymers, acid-activated inorganic polymers not only have superior physical properties but also have low pH values ​​and good durability, which makes acid-activated inorganic polymers applicable to a wider range of fields. However, due to the slow solidification of acid-activated inorganic polymers at room temperature, it often takes several days to reach the construction strength. In addition, due to the violent reaction during the stirring process, a large amount of heat is generated, and the slurry flowability is also poor. These shortcomings have caused great difficulties in actual construction. In order to alleviate the above defects, the setting time of phosphate-based inorganic polymers is greatly reduced by modifying the precursors and activators, the working performance of phosphate-based inorganic polymers is improved, and the early strength is increased. However, the shrinkage rate of phosphate-based inorganic polymers is much higher than that of silicate cement, especially under the condition of high water-cement ratio to meet the high fluidity of inorganic polymers, the shrinkage rate is higher. However, the high shrinkage of phosphoric acid-based inorganic polymers will seriously affect their application in practical engineering. Therefore, a modified phosphoric acid-based inorganic polymer, a preparation method and an application are urgently needed. Summary of the invention

[0004] In view of the problems of the prior art, the present invention provides a method for preparing a modified phosphoric acid-based inorganic polymer, comprising the following steps:

[0005] A method for preparing a modified phosphoric acid-based inorganic polymer comprises the following steps:

[0006] S1: mixing and stirring a modifier, active calcium oxide and metakaolin to obtain a powder raw material, and then mixing phosphoric acid, aluminum dihydrogen phosphate and water to obtain a liquid raw material; mixing and stirring the powder raw material and the liquid raw material to obtain an inorganic polymer slurry;

[0007] S2: pouring the inorganic polymer slurry obtained in S1 into a mold to form a sample, and then curing the sample to obtain a modified phosphoric acid-based inorganic polymer.

[0008] Furthermore, the chemical composition and weight percentage of the modifier in S1 are as follows: CaO is 65.5% to 72.7%, SO3 is 17.7% to 24.9%, SiO2 is 2.3% to 3.4%, Al2O3 is 2.3% to 3.0%, MgO is 0.9% to 1.8%, and Fe2O3 is 0.7% to 1.0%.

[0009] Furthermore, the stirring time described in S1 is 6 to 14 minutes.

[0010] Furthermore, the curing described in S2 is standard curing at a temperature of 18 to 22°C or steam curing at a temperature of 40 to 60°C.

[0011] Furthermore, the phosphoric acid described in S1 is industrial phosphoric acid with a mass concentration of 85%.

[0012] A modified phosphate-based inorganic polymer comprises: 47.3 to 50.6 parts of metakaolin, 3.3 parts of active calcium oxide, 1.7 to 5 parts of a modifier, 35.5 to 44.4 parts of phosphoric acid, 0 to 8.9 parts of aluminum dihydrogen phosphate, and the ratio of the weight of water to the weight of the powder raw material is 0.5 to 1.2.

[0013] The weight of water is the water added to the test, and the water contained in the phosphoric acid and aluminum dihydrogen phosphate solutions.

[0014] The invention discloses an application of a modified phosphoric acid-based inorganic polymer, wherein the modified phosphoric acid-based inorganic polymer is applied in the preparation of the phosphoric acid-based inorganic polymer.

[0015] Technical Effects

[0016] (1) Product: The modified phosphoric acid-based inorganic polymer provided by the present invention improves the compressive strength and shrinkage performance of the inorganic polymer by adding a modifier. The inorganic polymer prepared by the present invention has a 28-day compressive strength of 23.0 to 29.1 MPa, a setting time of 48 to 77 hours, and a shrinkage rate of 3400 to 6046.4×10 -6 .

[0017] (2) Advantages of the preparation method: The preparation method of a modified phosphate-based inorganic polymer provided by the present invention adopts a modifier composed of quicklime and calcium sulfate as the main phases as the modifier of the inorganic polymer, so that the mechanical properties of the inorganic polymer are improved and the shrinkage rate of the inorganic polymer is reduced; and in the preparation method, the curing method of the inorganic polymer can be either standard curing to meet the application requirements of actual engineering site construction, or steam curing to meet the preparation requirements of some prefabricated components used in acidic waste liquid discharge pipelines.

[0018] (3) Application: The modified phosphate-based inorganic polymer provided by the present invention is an effective way to realize the utilization of phosphate-based inorganic polymers and improve the ecological environment when the high shrinkage of the inorganic polymer affects its effective application.

[0019] Attached pictures

[0020] In order to more clearly illustrate the technical solutions of the exemplary embodiments of the present invention, the following briefly introduces the drawings required for use in the embodiments. It should be understood that the following drawings only illustrate certain embodiments of the present invention and should not be regarded as limiting the scope. For ordinary technicians in this field, other relevant drawings can be obtained based on these drawings without creative work. In the drawings,

[0021] Figure 1 1 is a SEM picture of the unmodified phosphoric acid-based inorganic polymer of comparative example 1 of the present invention at different magnifications after standard curing for 28 days.

[0022] Figure 2 1 and 1 are SEM images of the modified phosphate-based inorganic polymer of Example 2 of the present invention at different magnifications after 28 days of standard curing. DETAILED DESCRIPTION

[0023] The following will be combined with Examples 1 to 6 of the present invention, Comparative Examples 1 to 2 and the accompanying drawings to clearly and completely describe the technical solution of the present invention. It is obvious that the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0024] Example 1

[0025] S1: First, prepare 50.6 parts of metakaolin, 3.3 parts of active calcium oxide, 1.7 parts of modifier, 40 parts of phosphoric acid, and 4.4 parts of aluminum dihydrogen phosphate according to weight, and the ratio of the weight of water to the weight of the powder raw material is 0.8. Stir the prepared metakaolin, active calcium oxide and modifier in a cement mortar mixer for 1 minute until they are evenly mixed to obtain a powder raw material, and then add the prepared phosphoric acid, aluminum dihydrogen phosphate and water to the powder raw material and stir slowly for 6 minutes, and then stir quickly for 6 minutes to form an inorganic polymer slurry;

[0026] S2: Pour the inorganic polymer slurry obtained in S1 into a 40×40×40mm 3 The modified phosphoric acid-based inorganic polymer is formed in a mold to obtain a compressive strength test specimen, and then the specimen is placed in a humidity>90% and a temperature of 20±2°C for curing for 7 to 28 days.

[0027] The inorganic polymer slurry obtained in S1 was quickly poured into a 40×40×160 mm 3The modified phosphate-based inorganic polymer shrinkage test specimen is formed in a mold to obtain the modified phosphate-based inorganic polymer shrinkage test specimen, and then the obtained specimen is placed in a humidity>90% and a temperature of 20±2°C for curing for 7 days. After demolding, the specimen is transferred to a shrinkage curing box with a temperature of 20±2°C and a relative humidity of (60±5)% for curing for 28 days.

[0028] The modified phosphoric acid-based inorganic polymer obtained in Example 1 was subjected to a compressive strength test with reference to the "Test Method for Cement Mortar Strength", and the compressive strength of the inorganic polymer sample at the 7-day and 28-day curing ages was measured to be 19.1 MPa and 24.5 MPa, respectively. The initial and final setting times of the phosphoric acid-based inorganic polymer were measured with reference to the "Test Method for Cement Standard Consistency Water Consumption, Setting Time, and Stability", and were 65 h and 77 h, respectively. The shrinkage properties of the phosphoric acid-based inorganic polymer were measured with reference to the "Standard Test Method for Basic Properties of Building Mortar", and the shrinkage rate of the phosphoric acid-based inorganic polymer at 28 days was 6046.4×10 -6 .

[0029] Example 2

[0030] S1: First, prepare 49 parts of metakaolin, 3.3 parts of active calcium oxide, 3.3 parts of modifier, 40 parts of phosphoric acid, and 4.4 parts of aluminum dihydrogen phosphate according to weight, and the ratio of the weight of water to the weight of the powder raw material is 0.8. Stir the prepared metakaolin, active calcium oxide and modifier in a cement mortar mixer for 1 minute until they are evenly mixed to obtain a powder raw material, and then add the prepared phosphoric acid, aluminum dihydrogen phosphate and water to the powder raw material and stir slowly for 6 minutes, and then stir quickly for 6 minutes to form an inorganic polymer slurry;

[0031] S2: Pour the inorganic polymer slurry obtained in S1 into a 40×40×40mm 3 The inorganic polymer slurry obtained in S1 is quickly poured into a 40×40×160mm 3 The modified phosphate-based inorganic polymer shrinkage test specimen is formed in a mold to obtain the modified phosphate-based inorganic polymer shrinkage test specimen, and then the obtained specimen is placed in a humidity>90% and a temperature of 20±2°C for curing for 7 days. After demolding, the specimen is transferred to a shrinkage curing box with a temperature of 20±2°C and a relative humidity of (60±5)% for curing for 28 days.

[0032] The modified phosphate-based inorganic polymer obtained in Example 2 was subjected to a compressive strength test with reference to the "Test Method for Cement Mortar Strength", and the compressive strength of the inorganic polymer sample at the 7-day and 28-day curing ages was measured to be 20.3 MPa and 29.1 MPa, respectively; the initial setting and final setting times of the phosphate-based inorganic polymer were measured with reference to the "Test Method for Cement Standard Consistency Water Consumption, Setting Time, and Stability", and were 62 h and 71 h, respectively; the shrinkage properties of the phosphate-based inorganic polymer were measured with reference to the "Standard Test Method for Basic Properties of Building Mortar", and the shrinkage rate of the phosphate-based inorganic polymer at 28 days was 5718.5×10 -6 .

[0033] from Figure 2 It can be found that when the modifier replaces 6% of metakaolin, the microstructure of the modified inorganic polymer still contains unreacted powder particles, cracks and pores in addition to the inorganic polymer gel matrix, but the structure is more compact and the porosity and size are significantly reduced compared to the control. This is also the main reason why the addition of the modifier leads to an increase in the compressive strength of the inorganic polymer.

[0034] Example 3

[0035] S1: First, prepare 47.3 parts of metakaolin, 3.3 parts of active calcium oxide, 5 parts of modifier, 40 parts of phosphoric acid, and 4.4 parts of aluminum dihydrogen phosphate according to weight, and the ratio of the weight of water to the weight of the powder raw material is 0.8. Stir the prepared metakaolin, active calcium oxide and modifier in a cement mortar mixer for 1 minute until they are evenly mixed to obtain a powder raw material, and then add the prepared phosphoric acid, aluminum dihydrogen phosphate and water to the powder raw material and stir slowly for 6 minutes, and then stir quickly for 6 minutes to form an inorganic polymer slurry;

[0036] S2: Pour the inorganic polymer slurry obtained in S1 into a 40×40×40mm 3 The modified phosphoric acid-based inorganic polymer is formed in a mold to obtain a compressive strength test specimen, and then the specimen is placed in a humidity>90% and a temperature of 20±2°C for curing for 7 to 28 days.

[0037] The inorganic polymer slurry obtained in S1 was quickly poured into a 40×40×160 mm 3 The modified phosphate-based inorganic polymer shrinkage test specimen is formed in a mold to obtain the modified phosphate-based inorganic polymer shrinkage test specimen, and then the obtained specimen is placed in a humidity>90% and a temperature of 20±2°C for curing for 7 days. After demolding, the specimen is transferred to a shrinkage curing box with a temperature of 20±2°C and a relative humidity of (60±5)% for curing for 28 days.

[0038] The modified phosphoric acid-based inorganic polymer obtained in Example 3 was subjected to a compressive strength test. Referring to the "Test Method for Cement Mortar Strength", the compressive strength of the inorganic polymer sample at the 7-day and 28-day curing ages was measured to be 18.0 MPa and 23.7 MPa, respectively. Referring to the "Test Method for Cement Standard Consistency Water Consumption, Setting Time, and Stability", the initial setting and final setting times of the phosphoric acid-based inorganic polymer were measured to be 57 h and 70 h, respectively. Referring to the "Standard Test Method for Basic Performance of Building Mortar", the shrinkage performance of the phosphoric acid-based inorganic polymer was measured, and the shrinkage rate of the phosphoric acid-based inorganic polymer at 28 days was 4821.4×10 -6 .

[0039] Example 4

[0040] S1: First, prepare 50.6 parts of metakaolin, 3.3 parts of active calcium oxide, 1.7 parts of modifier, 35.5 parts of phosphoric acid, and 8.9 parts of aluminum dihydrogen phosphate according to weight, and the ratio of the weight of water to the weight of the powder raw material is 0.8. Stir the prepared metakaolin, active calcium oxide and modifier in a cement mortar mixer for 1 minute until they are evenly mixed to obtain a powder raw material, and then add the prepared phosphoric acid, aluminum dihydrogen phosphate and water to the powder raw material and stir slowly for 6 minutes, and then stir quickly for 6 minutes to form an inorganic polymer slurry;

[0041] S2: Pour the inorganic polymer slurry obtained in S1 into a 40×40×40mm 3 The modified phosphoric acid-based inorganic polymer is formed in a mold to obtain a compressive strength test specimen, and then the specimen is placed in a humidity>90% and a temperature of 20±2°C for curing for 7 to 28 days.

[0042] The inorganic polymer slurry obtained in S1 was quickly poured into a 40×40×160 mm 3 The modified phosphate-based inorganic polymer shrinkage test specimen is formed in a mold to obtain the modified phosphate-based inorganic polymer shrinkage test specimen, and then the obtained specimen is placed in a humidity>90% and a temperature of 20±2°C for curing for 7 days. After demolding, the specimen is transferred to a shrinkage curing box with a temperature of 20±2°C and a relative humidity of (60±5)% for curing for 28 days.

[0043] The modified phosphate-based inorganic polymer obtained in Example 4 was tested for compressive strength with reference to the "Test Method for Cement Mortar Strength", and the compressive strength of the inorganic polymer sample at the 7-day and 28-day curing age was measured to be 18.6 MPa and 23.0 MPa, respectively; the initial setting and final setting times of the phosphate-based inorganic polymer were measured with reference to the "Test Method for Cement Standard Consistency Water Consumption, Setting Time, and Stability", and were 60 h and 73 h, respectively; the shrinkage properties of the phosphate-based inorganic polymer were measured with reference to the "Standard Test Method for Basic Properties of Building Mortar", and the shrinkage rate of the phosphate-based inorganic polymer at 28 days was 4400.1×10 -6 .

[0044] Example 5

[0045] S1: First, prepare 49 parts of metakaolin, 3.3 parts of active calcium oxide, 3.3 parts of modifier, 35.5 parts of phosphoric acid, and 8.9 parts of aluminum dihydrogen phosphate according to weight, and the ratio of the weight of water to the weight of the powder raw material is 0.8. Stir the prepared metakaolin, active calcium oxide and modifier in a cement mortar mixer for 1 minute until they are evenly mixed to obtain a powder raw material, and then add the prepared phosphoric acid, aluminum dihydrogen phosphate and water to the powder raw material and stir slowly for 6 minutes, and then stir quickly for 6 minutes to form an inorganic polymer slurry;

[0046] S2: Pour the inorganic polymer slurry obtained in S1 into a 40×40×40mm 3 The modified phosphoric acid-based inorganic polymer is formed in a mold to obtain a compressive strength test specimen, and then the specimen is placed in a humidity>90% and a temperature of 20±2°C for curing for 7 to 28 days.

[0047] The inorganic polymer slurry obtained in S1 was quickly poured into a 40×40×160 mm 3 The modified phosphate-based inorganic polymer shrinkage test specimen is formed in a mold to obtain the modified phosphate-based inorganic polymer shrinkage test specimen, and then the obtained specimen is placed in a humidity>90% and a temperature of 20±2°C for curing for 7 days. After demolding, the specimen is transferred to a shrinkage curing box with a temperature of 20±2°C and a relative humidity of (60±5)% for curing for 28 days.

[0048] The modified phosphate-based inorganic polymer obtained in Example 5 was subjected to a compressive strength test with reference to the "Test Method for Cement Mortar Strength", and the compressive strength of the inorganic polymer sample at the 7-day and 28-day curing ages was measured to be 19.2 MPa and 25.6 MPa, respectively. The initial and final setting times of the phosphate-based inorganic polymer were measured with reference to the "Test Method for Cement Standard Consistency Water Consumption, Setting Time, and Stability", and were 53 h and 73 h, respectively. The shrinkage properties of the phosphate-based inorganic polymer were measured with reference to the "Standard Test Method for Basic Properties of Building Mortar", and the shrinkage rate of the phosphate-based inorganic polymer at 28 days was 3712.8 × 10 -6 .

[0049] Example 6

[0050] S1: First, prepare 47.3 parts of metakaolin, 3.3 parts of active calcium oxide, 5 parts of modifier, 35.5 parts of phosphoric acid, and 8.9 parts of aluminum dihydrogen phosphate according to weight, and the ratio of the weight of water to the weight of the powder raw material is 0.8. Stir the prepared metakaolin, active calcium oxide and modifier in a cement mortar mixer for 1 minute until they are evenly mixed to obtain a powder raw material, and then add the prepared phosphoric acid, aluminum dihydrogen phosphate and water to the powder raw material and stir slowly for 6 minutes, and then stir quickly for 6 minutes to form an inorganic polymer slurry;

[0051] S2: Pour the inorganic polymer slurry obtained in S1 into a 40×40×40mm 3 The inorganic polymer slurry obtained in S1 is quickly poured into a 40×40×160mm 3 The modified phosphate-based inorganic polymer shrinkage test specimen is formed in a mold to obtain the modified phosphate-based inorganic polymer shrinkage test specimen, and then the obtained specimen is placed in a humidity>90% and a temperature of 20±2°C for curing for 7 days. After demolding, the specimen is transferred to a shrinkage curing box with a temperature of 20±2°C and a relative humidity of (60±5)% for curing for 28 days.

[0052] The modified phosphoric acid-based inorganic polymer obtained in Example 6 was subjected to a compressive strength test with reference to the "Test Method for Cement Mortar Strength", and the compressive strength of the inorganic polymer sample at the 7-day and 28-day curing ages was measured to be 21.9 MPa and 24.8 MPa, respectively. The initial setting and final setting times of the phosphoric acid-based inorganic polymer were measured with reference to the "Test Method for Water Consumption, Setting Time and Stability of Cement Standard Consistency" to be 48 h and 72 h, respectively. The shrinkage properties of the phosphoric acid-based inorganic polymer were measured with reference to the "Standard Test Method for Basic Properties of Building Mortar", and the shrinkage rate of the phosphoric acid-based inorganic polymer at 28 days was 3400.0×10 -6 .

[0053] Comparative Example 1

[0054] S1: First, prepare 52.3 parts of metakaolin, 3.3 parts of active calcium oxide, 0 parts of modifier, 40 parts of phosphoric acid, and 4.4 parts of aluminum dihydrogen phosphate according to weight, and the ratio of the weight of water to the weight of the powder raw material is 0.8. Stir the prepared metakaolin, active calcium oxide and modifier in a cement mortar mixer for 1 minute until they are evenly mixed to obtain a powder raw material, and then add the prepared phosphoric acid, aluminum dihydrogen phosphate and water to the powder raw material and stir slowly for 6 minutes, and then stir quickly for 6 minutes to form an inorganic polymer slurry;

[0055] S2: Pour the inorganic polymer slurry obtained in S1 into a 40×40×40mm 3The modified phosphoric acid-based inorganic polymer is formed in a mold to obtain a compressive strength test specimen, and then the specimen is placed in a humidity>90% and a temperature of 20±2°C for curing for 7 to 28 days.

[0056] The inorganic polymer slurry obtained in S1 was quickly poured into a 40×40×160 mm 3 The modified phosphate-based inorganic polymer shrinkage test specimen is formed in a mold to obtain the modified phosphate-based inorganic polymer shrinkage test specimen, and then the obtained specimen is placed in a humidity>90% and a temperature of 20±2°C for curing for 7 days. After demolding, the specimen is transferred to a shrinkage curing box with a temperature of 20±2°C and a relative humidity of (60±5)% for curing for 28 days.

[0057] The modified phosphate-based inorganic polymer obtained in Comparative Example 1 was subjected to a compressive strength test with reference to the "Test Method for Cement Mortar Strength", and the compressive strength of the inorganic polymer sample at 7 days and 28 days of curing age was measured to be 15.7 MPa and 20.6 MPa, respectively; the initial and final setting times of the phosphate-based inorganic polymer were measured with reference to the "Test Method for Cement Standard Consistency Water Consumption, Setting Time, and Stability", and were 75 h and 85 h, respectively; the shrinkage properties of the phosphate-based inorganic polymer were measured with reference to the "Standard Test Method for Basic Properties of Building Mortar", and the shrinkage rate of the phosphate-based inorganic polymer at 28 days was 6499.1×10 -6 .

[0058] from Figure 1 It can be seen that in the microstructure of the inorganic polymer, inorganic polymer gel formed by polymerization reaction, unreacted kaolin, active calcium oxide or modifier powder particles, as well as microcracks and pores distributed in the inorganic polymer matrix can be observed, and the structure of the inorganic polymer is relatively loose.

[0059] Comparative Example 2

[0060] S1: First, prepare 52.3 parts of metakaolin, 3.3 parts of active calcium oxide, 0 parts of modifier, 35.5 parts of phosphoric acid, and 8.9 parts of aluminum dihydrogen phosphate according to weight, and the ratio of the weight of water to the weight of the powder raw material is 0.8. Stir the prepared metakaolin, active calcium oxide and modifier in a cement mortar mixer for 1 minute until they are evenly mixed to obtain a powder raw material, and then add the prepared phosphoric acid, aluminum dihydrogen phosphate and water to the powder raw material and stir slowly for 6 minutes, and then stir quickly for 6 minutes to form an inorganic polymer slurry;

[0061] S2: Pour the inorganic polymer slurry obtained in S1 into a 40×40×40mm 3 The modified phosphoric acid-based inorganic polymer is formed in a mold to obtain a compressive strength test specimen, and then the specimen is placed in a humidity>90% and a temperature of 20±2°C for curing for 7 to 28 days.

[0062] The inorganic polymer slurry obtained in S1 was quickly poured into a 40×40×160 mm 3 The modified phosphate-based inorganic polymer shrinkage test specimen is formed in a mold to obtain the modified phosphate-based inorganic polymer shrinkage test specimen, and then the obtained specimen is placed in a humidity>90% and a temperature of 20±2°C for curing for 7 days. After demolding, the specimen is transferred to a shrinkage curing box with a temperature of 20±2°C and a relative humidity of (60±5)% for curing for 28 days.

[0063] The modified phosphate-based inorganic polymer obtained in Comparative Example 2 was subjected to a compressive strength test with reference to the "Test Method for Cement Mortar Strength", and the compressive strength of the inorganic polymer sample at 7 days and 28 days of curing age was measured to be 14.3 MPa and 19.3 MPa, respectively; the initial setting and final setting times of the phosphate-based inorganic polymer were measured with reference to the "Test Method for Cement Standard Consistency Water Consumption, Setting Time, and Stability", and were 72 h and 87 h, respectively; the shrinkage properties of the phosphate-based inorganic polymer were measured with reference to the "Standard Test Method for Basic Properties of Building Mortar", and the shrinkage rate of the phosphate-based inorganic polymer at 28 was 5700×10 -6 .

[0064] In order to further compare the effect of the present invention, under the same preparation process conditions as the embodiments of the present invention, inorganic polymers without modifiers were used as comparisons, and the setting time, compressive strength and shrinkage of the products were compared. The results are listed in Tables 1 and 2.

[0065] Table 1 Parameter comparison table of Examples 1 to 6 and Comparative Examples 1 to 2

[0066]

[0067]

[0068] Table 2 Comparison of relevant parameters of Examples 1 to 6 and Comparative Examples 1 to 2

[0069]

[0070] In Tables 1 to 2, in Example 1, Example 2 and Example 3, compared with Comparative Example 1, the amount of aluminum dihydrogen phosphate in the activator remains unchanged (aluminum dihydrogen phosphate: phosphoric acid = 1:9), the ratio of the weight of water to the weight of other solids remains unchanged at 0.8, the amount of active calcium oxide remains unchanged, and only 3%, 6% and 9% of the metakaolin are replaced by the modifier. The 28-day compressive strength of the phosphoric acid-based inorganic polymer is increased by 18.9%, 41.2% and 15.0%, respectively, while the 28-day shrinkage rate is reduced by 6.7%, 12.1% and 25.8%, respectively.

[0071] In Examples 4, 5 and 6 in Tables 1 to 2, compared with Comparative Example 2, the amount of aluminum dihydrogen phosphate in the activator remains unchanged (aluminum dihydrogen phosphate: phosphoric acid = 2:8), the ratio of the weight of water to the weight of other solids remains unchanged at 0.8, the amount of active calcium oxide remains unchanged, and only 3%, 6% and 9% of the metakaolin are replaced by the modifier. The 28-day compressive strength of the phosphoric acid-based inorganic polymer is increased by 16.1%, 32.6% and 26.5%, respectively, while the 28-day shrinkage rate is reduced by 22.8%, 34.8% and 40.4%, respectively.

[0072] The modified phosphate-based inorganic polymer obtained by the preparation method of the modified phosphate-based inorganic polymer provided by the present invention has high compressive strength and significantly improved mechanical properties. Compared with traditional inorganic polymers, the compressive strength is significantly improved, making it more suitable for bearing larger loads and pressures. The setting time of the modified phosphate-based inorganic polymer is controlled within 48 to 77 hours. This moderate setting time is conducive to control and operation during the construction process, while ensuring the early strength development of the material.

[0073] The present invention provides a method for preparing a modified phosphoric acid-based inorganic polymer, wherein the selection of a modifier (with quicklime and calcium sulfate as the main phase) reduces the drying shrinkage rate of the inorganic polymer to 3400-6046.4×10 -6 , effectively reducing cracks and deformation caused by shrinkage during use, improving the stability and durability of the structure, and the inorganic polymer provided by the present invention can be selected for standard curing or steam curing according to actual engineering needs. Standard curing is suitable for most engineering sites, while steam curing is particularly suitable for specific applications that require rapid hardening and high early strength.

[0074] The preparation method of a modified phosphate-based inorganic polymer provided by the present invention can broaden the application. The modified phosphate-based inorganic polymer has made a breakthrough in the problem of high shrinkage, which not only improves the environmental adaptability of the material, but also provides an effective material selection for ecological environmental protection. The addition of the modifier and the optimization of the preparation method reduce the production cost and improve the cost performance of the material, so that the inorganic polymer of the present invention has stronger competitiveness in the market. The present invention not only improves the performance of the inorganic polymer, but also actively responds to the call for sustainable development. By using the modifier, the impact on the environment is reduced, and the green development of the building materials industry is promoted.

Claims

1. A method for preparing a modified phosphoric acid-based inorganic polymer, characterized in that: The following steps are involved: S1: mixing and stirring a modifier, active calcium oxide and metakaolin to obtain a powder raw material, and then mixing phosphoric acid, aluminum dihydrogen phosphate and water to obtain a liquid raw material; mixing and stirring the powder raw material and the liquid raw material to obtain an inorganic polymer slurry; S2: pouring the inorganic polymer slurry obtained in S1 into a mold to form a sample, and then curing the sample to obtain a modified phosphoric acid-based inorganic polymer.

2. The method for preparing a modified phosphoric acid-based inorganic polymer according to claim 1, characterized in that: The chemical composition and weight percentage of the modifier in S1 are as follows: CaO is 65.5% to 72.7%, SO3 is 17.7% to 24.9%, SiO2 is 2.3% to 3.4%, Al2O3 is 2.3% to 3.0%, MgO is 0.9% to 1.8%, and Fe2O3 is 0.7% to 1.0%.

3. The method for preparing a modified phosphoric acid-based inorganic polymer according to claim 1, characterized in that: The stirring time described in S1 is 6 to 14 minutes.

4. The method for preparing a modified phosphoric acid-based inorganic polymer according to claim 1, characterized in that: The curing temperature described in S2 is standard curing at 18 to 22°C or steam curing at 40 to 60°C.

5. The method for preparing a modified phosphoric acid-based inorganic polymer according to claim 1, characterized in that: The phosphoric acid described in S1 is industrial phosphoric acid with a mass concentration of 85%.

6. A modified phosphoric acid-based inorganic polymer obtained by the preparation method according to any one of claims 1 to 5, characterized in that: The modified phosphate-based inorganic polymer comprises: 47.3 to 50.6 parts of metakaolin, 3.3 parts of active calcium oxide, 1.7 to 5 parts of a modifier, 35.5 to 44.4 parts of phosphoric acid, 0 to 8.9 parts of aluminum dihydrogen phosphate, and the ratio of the weight of water to the weight of the powder raw material is 0.5 to 1.2; The weight of water is the water added to the test, and the water contained in the phosphoric acid and aluminum dihydrogen phosphate solutions.

7. The use of a modified phosphoric acid-based inorganic polymer according to claim 6, characterized in that: The modified phosphoric acid-based inorganic polymer is used in the preparation of phosphoric acid-based inorganic polymer.