Rust-resistant high-strength special grouting mortar and preparation method thereof
The rust-resistant high-strength special grouting mortar addresses corrosion and mechanical strength issues in reinforced concrete structures by optimizing material ratios and distribution using advanced algorithms, providing enhanced durability and cost-effectiveness.
Patent Information
- Application Number
- CN202411248850.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Traditional anti-corrosion methods for steel bars in reinforced concrete structures are inadequate, especially in harsh environments, and existing grouting mortars fail to meet mechanical strength and durability requirements, leading to corrosion and structural failure.
A rust-resistant high-strength special grouting mortar is prepared using an adaptive hierarchical reaction control algorithm and multi-level adaptive dispersion algorithm to optimize material ratios and ensure uniform distribution, enhancing corrosion resistance and mechanical properties.
The mortar effectively prevents steel corrosion and improves mechanical strength, ensuring durability and long-term structural integrity under harsh conditions, while reducing material waste and construction costs.
Smart Images

Figure CN119080460A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of building materials, and in particular to a rust-resistant high-strength special grouting mortar and a preparation method thereof. Background Art
[0002] In modern construction projects, reinforced concrete is one of the most commonly used structural materials. However, reinforced concrete structures face many problems in practical applications, especially the corrosion of steel bars. The corrosion of steel bars not only reduces the mechanical properties of concrete structures, but also may lead to early failure of the structure, thus seriously threatening the safety and service life of buildings. Therefore, how to effectively prevent steel corrosion and extend the service life of reinforced concrete structures is an important research direction in the field of building materials technology.
[0003] First, traditional steel bar anti-corrosion methods mainly include the use of stainless steel bars, anti-corrosion coatings, and the addition of rust inhibitors to concrete. Although these methods can delay the corrosion of steel bars to a certain extent, their application also has obvious limitations. For example, although the use of stainless steel bars can effectively prevent corrosion, the cost is high and it is difficult to be widely used in large-scale projects; although the application of anti-corrosion coatings can provide a physical barrier, the coating is easily damaged during the construction process, thereby reducing the anti-corrosion effect; and traditional rust inhibitors are prone to failure in environments with high chloride ion concentrations due to their mechanism of action, and even cause local corrosion.
[0004] Secondly, in modern construction projects, with the increasing requirements for the durability of building structures, higher requirements are also placed on the mechanical properties of grouting mortar. Although traditional grouting mortar can meet the needs of general projects, its performance in mechanical properties, crack resistance, impact resistance, etc. is still unsatisfactory, especially under harsh environmental conditions, such as seaport terminals, offshore wind power foundations, etc., the performance of traditional grouting mortar is particularly insufficient. Under these environmental conditions, corrosive media such as moisture, chloride ions, and carbon dioxide can easily enter the surface of the steel bars through the pores of the mortar, accelerating the corrosion of the steel bars. In addition, due to the effect of shrinkage stress during the hardening process, traditional mortar is prone to microcracks, which further increase the risk of penetration of corrosive media, thereby reducing the anti-corrosion performance of the mortar.
[0005] Third, with the advancement of science and technology and the development of computer technology, more and more building materials research and development have begun to rely on algorithm optimization and simulation technology. Although some studies have tried to improve the performance of grouting mortar through optimization algorithms, these algorithms are mostly conventional algorithms, which are difficult to handle the complex and changeable actual construction environment, and there is still a lot of room for improvement in the uniform dispersion of materials and performance optimization. Especially in the composite application of multiple materials, how to achieve the optimal ratio and dispersion of materials through algorithms is a difficulty in current technology.
[0006] In summary, the existing technology still has many defects in preventing steel bar corrosion and improving the mechanical properties of grouting mortar: traditional anti-corrosion methods cannot fully solve the corrosion problem of steel bars in harsh environments, the mechanical properties of existing grouting mortars cannot meet the needs of high-strength engineering, and the existing optimization algorithms cannot fully optimize the material ratio and dispersion effect. Therefore, how to provide a rust-resistant high-strength special grouting mortar and its preparation method is a problem that technicians in this field need to solve urgently. Summary of the invention
[0007] One purpose of the present invention is to provide a rust-resistant high-strength special grouting mortar and a preparation method thereof. The present invention introduces an adaptive hierarchical reaction control algorithm and a multi-level adaptive dispersion algorithm, and describes in detail how to achieve the optimal ratio and uniform dispersion of materials in the mortar preparation process, which significantly improves the corrosion resistance and mechanical properties of the mortar, can effectively deal with the problem of steel bar corrosion, and has the advantages of strong durability, high protective performance and high construction efficiency.
[0008] A rust-resistant high-strength special grouting mortar and a preparation method thereof according to an embodiment of the present invention include the following steps:
[0009] S1. Weigh the PO52.5 ordinary Portland cement, silica fume, fly ash microbead powder, mineral powder, and quartz sand prepared in claim 1, conduct multiple experiments using an adaptive hierarchical reaction control algorithm, generate multiple ingredient combinations, and record relevant experimental data;
[0010] S2. Based on the experimental data obtained in S1, the optimization algorithm is used to evaluate the performance of each ingredient combination, select the ingredient combination with the best performance, and determine the final optimal ingredient ratio;
[0011] S3, weighing PO52.5 ordinary Portland cement, silica fume, fly ash microbead powder, mineral powder and quartz sand according to the determined optimal proportion of ingredients, and mixing these components evenly to prepare a dry powder mixture;
[0012] S4. The dry powder mixture is conveyed to the mixing bin by means of an auger or an elevator. When the conveying reaches 70%, the conveying is stopped, and PVA fiber, PC-1051 water reducing agent and defoaming agent are added. The remaining dry powder mixture is conveyed to the mixing bin.
[0013] S5, starting the mixer and the flying knife, using a multi-level adaptive dispersion algorithm to regulate the distribution of the PVA fibers, and completing uniform stirring of the slurry;
[0014] S6. After the stirring is completed, the slurry is tested and the physical and chemical properties are recorded;
[0015] S7. Based on the test results, use the slurry that meets the requirements for grouting construction and follow the prescribed steps.
[0016] Optionally, the S1 includes the following steps:
[0017] S11. Weigh the PO52.5 ordinary Portland cement, silica fume, fly ash microbead powder, mineral powder, and quartz sand prepared in claim 1, and record the mass M of each material respectively. i , where i = 1, 2, 3, 4, 5 correspond to cement, silica fume, fly ash microbead powder, mineral powder, quartz sand, and particle size d i , and the specific surface area S i , for the reaction rate R i (t) Calculation and optimization of material ratio;
[0018] S12, using the adaptive hierarchical reaction control algorithm, through multiple experiments to determine the hydration reaction rate R of each material i (t) and the degree of reaction E i (t) to generate multiple ingredient combinations and record related data:
[0019]
[0020] Among them, R i (t) represents material M i The hydration reaction rate at time t; A i is the material's reactive constant force; S i is the specific surface area of the material; d i is the average particle size of the material; n is the particle size influencing factor; θ(t') is the thermodynamic reaction angle of the material at time t'; is the time derivative of the thermodynamic reaction angle; δ is the thermodynamic nonlinear characteristic index; E a is the activation energy of the material; γ is the humidity correction coefficient; H is the ambient humidity; R is the gas constant; T is the reaction temperature; m is the nonlinear index of humidity influence;
[0021] S13, material M i According to particle size d i Divided into different levelsG j , in order to more accurately calculate the reaction rate R at each level i,j (t) and the degree of reaction E i,j (t), the reaction rate R of the material i,j (t) is calculated by the following formula:
[0022]
[0023] Among them, R i,j (t) represents the jth level material M i,j The hydration reaction rate at time t; A i,jis the reactivity constant of the j-th level material; S i,j is the specific surface area of the jth level material; d i,j is the particle size of the jth level material; θ j (t) is the thermodynamic reaction angle of the j-th level material; δ j E is the thermodynamic nonlinear characteristic index of the j-th level material; a,j is the activation energy of the jth level material; m j is the nonlinear index of humidity effect;
[0024] S14. At each grading stage G j After the end, based on the experimental data of the previous level, adjust the addition ratio P of the next level of materials i,j (t) and sequence S i,j (t), in order to optimize the subsequent reaction process, the addition ratio of the material P i,j (t+1) is determined by the following formula:
[0025]
[0026] Among them, P i,j (t) represents the proportion of the j-th level material added at time t; E i,j (t') represents the reaction degree of the j-th level material at time t'; It represents the cumulative sum of the reaction rate and reaction extent of all levels of materials at time t;
[0027] S15. After multiple rounds of experiments, calculate the global reaction effect of each level of material I total , integrate all experimental data, evaluate the comprehensive influence of different proportions on mortar performance, and the global reaction effect I total :
[0028]
[0029] Among them, I total Represents the comprehensive response performance of all materials during the entire experiment; σ i,j Contribution of material to compressive strength at level j;
[0030] S16. Determine the final optimal material ratio P by optimizing the objective function optimal :
[0031]
[0032] Among them, P optimal Indicates the optimal material ratio finally determined.
[0033] Optionally, S2 includes the following steps:
[0034] S21, according to the experimental data in claim 3, extract the hydration reaction rate R of each ingredient combination i (t), reaction degree E i (t) and compressive strength σ i , taking these data as input, we prepare for further optimization analysis;
[0035] S22, use weighted optimization algorithm to make preliminary evaluation on each ingredient combination, and the comprehensive performance index C i (t) is calculated by the following formula:
[0036]
[0037] Among them, C i (t) is the comprehensive performance index of ingredient combination i at time t; α, β, is the weighting coefficient of the optimization algorithm; R i (t) is the material M i The hydration reaction rate at time t; E i (t) is the material M i The degree of reaction; i For material M i The compressive strength;
[0038] S23. After the initial evaluation, the adaptive genetic algorithm is used to further optimize the ingredient combination and define the fitness function F(C i ) to evaluate the fitness of each combination, and the fitness function is based on the comprehensive performance index C i (t) Calculate:
[0039]
[0040] Among them, F(C i ) is the fitness value of ingredient combination i; max(C i (t)) is the highest comprehensive performance index among all ingredient combinations;
[0041] S24. In the adaptive genetic algorithm, crossover and mutation operations are used to generate new ingredient combinations P new (t); In each round, the crossover operation is performed using the following formula:
[0042] P new (t) = λ·P parent1 (t)+(1-λ)·P parent2 (t);
[0043] Among them, P new (t) is the ratio of the newly generated ingredient combination at time t; P parent1 (t) and Pparent2 (t is the selected parent ingredient combination; λ is the crossover factor, which controls the similarity between the new combination and the parent, and its value is between 0 and 1;
[0044] S25, the mutation operation adjusts the individual parameters of the newly generated combination according to the following formula:
[0045] P mutated (t) = P new (t)+∈·N(0,1);
[0046] Among them, P mutated (t) is the ratio of the mutated ingredient combination at time t; ∈ is the mutation intensity; N(0,1) is a random variable that obeys the normal distribution;
[0047] S26. After multiple rounds of crossover and mutation operations, calculate the comprehensive performance index C of the new ingredient combination generated in each round new (t), and recalculate the fitness value F)C new ), and finally select the ingredient combination with the highest fitness as the optimal ingredient ratio after optimization;
[0048] S27, the final optimized ingredient ratio P optimal Used in the next experiment or actual production.
[0049] Optionally, S3 includes the following steps:
[0050] S31, according to the best proportion of ingredients P determined in claim 4 optimal , weigh PO52.5 ordinary Portland cement M 1 、Silica fume M 2 、Fly ash microbead powder M 3 、Mineral powder M 4 and quartz sand M 5 , the mass of each material is weighed according to the optimal ratio determined in claim 4;
[0051] S32, after weighing, add PO52.5 ordinary Portland cement M 1 First add the dry powder mixer, then add silica fume M 2 、Fly ash microbead powder M 3 、Mineral powder M 4 and quartz sand M 5 ; The order of addition depends on the physical properties of the materials;
[0052] S33. During the mixing process, control the speed and time of the mixer to ensure that all materials are fully mixed and uniform to form a homogeneous dry powder mixture. The speed v of the mixer and the mixing time t m Determined by the results of the optimization algorithm to avoid delamination and aggregation of materials;
[0053] S34, after the mixing is completed, the uniformity of the mixture is detected, and the particle size distribution and specific surface area of the mixture are respectively detected using a particle size analyzer and a specific surface area measuring instrument;
[0054] S35. According to the test results, if it is found that the uniformity of the mixture does not meet the expected standard, adjust the speed and time of the mixer, and re-mix until the uniformity of the mixture meets the requirements. Re-testing is required after each adjustment;
[0055] S36. Package the final dry powder mixture and mark it with information such as material ratio, mixing time and mixer parameters to facilitate subsequent construction and quality control.
[0056] Optionally, S4 includes the following steps:
[0057] S41. Use an auger or an elevator to gradually convey the dry powder mixture prepared in claim 5 to a mixing bin. During the conveying process, control the conveying rate and conveying amount so that the dry powder mixture enters the mixing bin evenly to avoid local accumulation or uneven distribution in the mixing bin.
[0058] S42, when the dry powder mixture is conveyed to 70% of the total amount of the mixing bin, the conveying is suspended;
[0059] S43, after pausing the conveying, add PVA fiber, PC-1051 water reducing agent and defoaming agent in sequence; the order of adding additives is optimized through experiments to ensure that they can be evenly dispersed during the subsequent stirring process, and special attention is paid to the distribution uniformity of PVA fiber to ensure the crack resistance and toughness of the slurry;
[0060] S44. After adding PVA fiber, PC-1051 water reducing agent and defoaming agent, restart the auger or elevator to continue conveying the remaining 30% dry powder mixture to the mixing bin;
[0061] S45, after all the dry powder mixture is delivered, the stirring device in the stirring bin is started to fully mix all the components to form a homogeneous slurry;
[0062] S46. After the stirring is completed, the slurry is immediately tested. The test items include the fluidity, viscosity and uniformity of the slurry. According to the test results, if it is found that it does not meet the requirements, the stirring parameters need to be adjusted and the stirring should be repeated until the slurry reaches the expected standards.
[0063] Optionally, S5 includes the following steps:
[0064] S51, start the mixer and the flying knife to preliminarily mix the materials prepared in claim 6. At this time, the initial speed v of the mixer is s(0) and the initial cutting frequency f of the flying cutter c (0) Set as base value v base and f base ; S52, in the primary stirring stage, the multi-level adaptive dispersion algorithm is applied to monitor the viscosity η(t of the slurry and the distribution density ρ of the PVA fiber in real time PVA (t), stirring speed v s (t) and cutting frequency f c (t) Dynamic adjustment is performed according to the following formula:
[0065]
[0066]
[0067] Where η(t) represents the slurry viscosity at time t; ρ PVA (t) represents the distribution density of PVA fibers at time t; Ψ and Θ are adjustment coefficients;
[0068] S53, in the mid-term stirring stage, the multi-level adaptive dispersion algorithm gradually increases the stirring speed v according to the increase in slurry viscosity and the uniformity of fiber distribution. s (t) and cutting frequency f c (t) to further optimize the dispersion of PVA fibers:
[0069]
[0070] Among them, v opt and f opt is the optimal stirring speed and cutting frequency in the mid-term stage; Ψ and Θ are the adjustment coefficients; η max and ρ PVA,max are the maximum allowable viscosity of the slurry and the maximum allowable fiber distribution density;
[0071] S54. In the later stage of stirring, the multi-level adaptive dispersion algorithm adjusts the stirring speed and the cutting frequency to the final optimized state. The adjustment formula of the stirring speed and the cutting frequency is:
[0072]
[0073] Among them, v final and f final is the final stirring speed and cutting frequency in the later stage; Ψ and Θ are the adjustment coefficients; η target and ρ PVA,target They are the final target values of slurry viscosity and fiber distribution density;
[0074] S55. After the stirring is completed, the slurry is immediately tested, with a focus on the uniformity of the distribution of the PVA fibers and the overall viscosity and fluidity of the slurry. If the test results do not meet the standards, the stirring parameters are adjusted based on the feedback and the stirring is repeated until the expected standards are met.
[0075] The beneficial effects of the present invention are:
[0076] (1) The present invention proposes a rust-resistant high-strength special grouting mortar and a preparation method thereof. By adopting an adaptive hierarchical reaction control algorithm, the hydration reaction rate and reaction degree of each raw material in the mortar are accurately controlled, multiple ingredient combinations are generated and their performance is evaluated, thereby determining the optimal ingredient ratio. This method effectively improves the mechanical properties and corrosion resistance of the mortar, ensuring the high strength and durability of the final product.
[0077] (2) The present invention introduces a multi-level adaptive dispersion algorithm to dynamically adjust the stirring speed and cutting frequency during the mortar mixing process to ensure the uniform distribution of PVA fibers in the slurry. By real-time monitoring and regulation of the slurry viscosity and fiber distribution density, fiber aggregation and material stratification are avoided, and the uniformity and construction performance of the mortar are significantly improved, so that the mortar has excellent crack resistance and long-term protective effect in practical applications.
[0078] (3) The present invention significantly improves the corrosion resistance and mechanical strength of grouting mortar under harsh environmental conditions by optimizing the proportion of mortar ingredients and the mixing process. In particular, in an environment with high chloride ion concentration, the mortar effectively prevents steel corrosion through an inherent rust-proof mechanism, and while ensuring high strength, it prolongs the service life of the building structure, providing a more reliable and durable material option for modern construction projects.
[0079] (4) The present invention adopts intelligent optimization and control algorithms, which not only improves the overall performance of mortar, but also simplifies the traditional production process, reduces material waste and construction costs. Through the application of adaptive algorithms, the present invention realizes the optimization of the entire process from batching to mixing to final construction, effectively ensuring the consistency and stability of the product, and providing a cost-effective solution for construction projects. BRIEF DESCRIPTION OF THE DRAWINGS
[0080] The accompanying drawings are used to provide a further understanding of the present invention and constitute a part of the specification. Together with the embodiments of the present invention, they are used to explain the present invention and do not constitute a limitation of the present invention. In the accompanying drawings:
[0081] Figure 1 A flowchart of a rust-resistant high-strength special grouting mortar and a preparation method thereof proposed by the present invention;
[0082] Figure 2It is a schematic diagram of the flow of the adaptive hierarchical reaction control algorithm proposed by the present invention;
[0083] Figure 3 This is a flow chart of the multi-level adaptive decentralized algorithm proposed in the present invention. DETAILED DESCRIPTION
[0084] The present invention will now be described in further detail with reference to the accompanying drawings. These drawings are simplified schematic diagrams, which only illustrate the basic structure of the present invention in a schematic manner, and therefore only show the components related to the present invention.
[0085] refer to Figure 1-3 A rust-resistant high-strength special grouting mortar and a preparation method thereof, comprising the following steps:
[0086] S1. Weigh the PO52.5 ordinary Portland cement, silica fume, fly ash microbead powder, mineral powder, and quartz sand prepared in claim 1, conduct multiple experiments using an adaptive hierarchical reaction control algorithm, generate multiple ingredient combinations, and record relevant experimental data;
[0087] S2. Based on the experimental data obtained in S1, the optimization algorithm is used to evaluate the performance of each ingredient combination, select the ingredient combination with the best performance, and determine the final optimal ingredient ratio;
[0088] S3, weighing PO52.5 ordinary Portland cement, silica fume, fly ash microbead powder, mineral powder and quartz sand according to the determined optimal proportion of ingredients, and mixing these components evenly to prepare a dry powder mixture;
[0089] S4. The dry powder mixture is conveyed to the mixing bin by means of an auger or an elevator. When the conveying reaches 70%, the conveying is stopped, and PVA fiber, PC-1051 water reducing agent and defoaming agent are added. The remaining dry powder mixture is conveyed to the mixing bin.
[0090] S5, starting the mixer and the flying knife, using a multi-level adaptive dispersion algorithm to regulate the distribution of the PVA fibers, and completing uniform stirring of the slurry;
[0091] S6. After the stirring is completed, the slurry is tested and the physical and chemical properties are recorded;
[0092] S7. Based on the test results, use the slurry that meets the requirements for grouting construction and follow the prescribed steps.
[0093] In this implementation, S1 includes the following steps:
[0094] S11. Weigh the PO52.5 ordinary Portland cement, silica fume, fly ash microbead powder, mineral powder, and quartz sand prepared in claim 1, and record the mass M of each material respectively. i, where i = 1, 2, 3, 4, 5 correspond to cement, silica fume, fly ash microbead powder, mineral powder, quartz sand, and particle size d i , and the specific surface area S i , for the reaction rate R i (t) Calculation and optimization of material ratio;
[0095] S12, using the adaptive hierarchical reaction control algorithm, through multiple experiments to determine the hydration reaction rate R of each material i (t) and the degree of reaction E i (t) to generate multiple ingredient combinations and record related data:
[0096]
[0097] Among them, R i (t) represents material M i The hydration reaction rate at time t; A i is the material's reactive constant force; S i is the specific surface area of the material; d i is the average particle size of the material; n is the particle size influencing factor; θ(t') is the thermodynamic reaction angle of the material at time t'; is the time derivative of the thermodynamic reaction angle; δ is the thermodynamic nonlinear characteristic index; E a is the activation energy of the material; γ is the humidity correction coefficient; H is the ambient humidity; R is the gas constant; T is the reaction temperature; m is the nonlinear index of humidity influence;
[0098] S13, material M i According to particle size d i Divided into different levelsG j , in order to more accurately calculate the reaction rate R at each level i,j (t) and the degree of reaction E i,j (t), the reaction rate R of the material i,j (t) is calculated by the following formula:
[0099]
[0100] Among them, R i,j (t) represents the jth level material M i,j The hydration reaction rate at time t; A i,j is the reactivity constant of the j-th level material; S i,j is the specific surface area of the jth level material; d i,j is the particle size of the jth level material; θ j (t) is the thermodynamic reaction angle of the j-th level material; δ j E is the thermodynamic nonlinear characteristic index of the j-th level material;a,j is the activation energy of the jth level material; m j is the nonlinear index of humidity effect;
[0101] S14. At each grading stage G j After the end, based on the experimental data of the previous level, adjust the addition ratio P of the next level of materials i,j (t) and sequence S i,j (t), in order to optimize the subsequent reaction process, the addition ratio of the material P i,j (t+1) is determined by the following formula:
[0102]
[0103] Among them, P i,j (t) represents the proportion of the j-th level material added at time t; E i,j (t') represents the reaction degree of the j-th level material at time t'; It represents the cumulative sum of the reaction rate and reaction extent of all levels of materials at time t;
[0104] S15. After multiple rounds of experiments, calculate the global reaction effect of each level of material I total , integrate all experimental data, evaluate the comprehensive influence of different proportions on mortar performance, and the global reaction effect I total :
[0105]
[0106] Among them, I total Represents the comprehensive response performance of all materials during the entire experiment; σ i,j Contribution of material to compressive strength at level j;
[0107] S16. Determine the final optimal material ratio P by optimizing the objective function optimal :
[0108]
[0109] Among them, P optimal Indicates the optimal material ratio finally determined.
[0110] In this implementation, S2 includes the following steps:
[0111] S21, according to the experimental data in claim 3, extract the hydration reaction rate R of each ingredient combination i (t), reaction degree E i (t) and compressive strength σ i , taking these data as input, we prepare for further optimization analysis;
[0112] S22, use weighted optimization algorithm to make preliminary evaluation on each ingredient combination, and the comprehensive performance index C i (t) is calculated by the following formula:
[0113]
[0114] Among them, C i (t) is the comprehensive performance index of ingredient combination i at time t; α, β, is the weighting coefficient of the optimization algorithm; R i (t) is the material M i The hydration reaction rate at time t; E i (t) is the material M i The degree of reaction; i For material M i The compressive strength;
[0115] S23. After the initial evaluation, the adaptive genetic algorithm is used to further optimize the ingredient combination and define the fitness function F(C i ) to evaluate the fitness of each combination, and the fitness function is based on the comprehensive performance index C i (t) Calculate:
[0116]
[0117] Among them, F(C i ) is the fitness value of ingredient combination i; max(C i (t)) is the highest comprehensive performance index among all ingredient combinations;
[0118] S24. In the adaptive genetic algorithm, crossover and mutation operations are used to generate new ingredient combinations P new (t); In each round, the crossover operation is performed using the following formula:
[0119] P new (t) = λ·P parent1 (t)+(1-λ)·P parent2 (t);
[0120] Among them, P new (t) is the ratio of the newly generated ingredient combination at time t; P parent1 (t) and P parent2 (t is the selected parent ingredient combination; λ is the crossover factor, which controls the similarity between the new combination and the parent, and the value is between 0 and 1;
[0121] S25, the mutation operation adjusts the individual parameters of the newly generated combination according to the following formula:
[0122] Pmutated (t) = P new (t)+∈·N(0,1);
[0123] Among them, P mutated (t) is the ratio of the mutated ingredient combination at time t; ∈ is the mutation intensity; N(0,1) is a random variable that obeys the normal distribution;
[0124] S26. After multiple rounds of crossover and mutation operations, calculate the comprehensive performance index C of the new ingredient combination generated in each round new (t), and recalculate the fitness value F(C new ), and finally select the ingredient combination with the highest fitness as the optimal ingredient ratio after optimization;
[0125] S27, the final optimized ingredient ratio P optimal Used in the next experiment or actual production.
[0126] In this implementation, S3 includes the following steps:
[0127] S31, according to the best proportion of ingredients P determined in claim 4 optimal , weigh PO52.5 ordinary Portland cement M 1 、Silica fume M 2 、Fly ash microbead powder M 3 、Mineral powder M 4 and quartz sand M 5 , the mass of each material is weighed according to the optimal ratio determined in claim 4;
[0128] S32, after weighing, add PO52.5 ordinary Portland cement M 1 First add the dry powder mixer, then add silica fume M 2 、Fly ash microbead powder M 3 、Mineral powder M 4 and quartz sand M 5 ; The order of addition depends on the physical properties of the materials;
[0129] S33. During the mixing process, control the speed and time of the mixer to ensure that all materials are fully mixed and uniform to form a homogeneous dry powder mixture. The speed v of the mixer and the mixing time t m Determined by the results of the optimization algorithm to avoid delamination and aggregation of materials;
[0130] S34, after the mixing is completed, the uniformity of the mixture is detected, and the particle size distribution and specific surface area of the mixture are respectively detected using a particle size analyzer and a specific surface area measuring instrument;
[0131] S35. According to the test results, if it is found that the uniformity of the mixture does not meet the expected standard, adjust the speed and time of the mixer, and re-mix until the uniformity of the mixture meets the requirements. Re-testing is required after each adjustment;
[0132] S36. Package the final dry powder mixture and mark it with information such as material ratio, mixing time and mixer parameters to facilitate subsequent construction and quality control.
[0133] In this implementation, S4 includes the following steps:
[0134] S41. Use an auger or an elevator to gradually convey the dry powder mixture prepared in claim 5 to a mixing bin. During the conveying process, control the conveying rate and conveying amount so that the dry powder mixture enters the mixing bin evenly to avoid local accumulation or uneven distribution in the mixing bin.
[0135] S42, when the dry powder mixture is conveyed to 70% of the total amount of the mixing bin, the conveying is suspended;
[0136] S43, after pausing the conveying, add PVA fiber, PC-1051 water reducing agent and defoaming agent in sequence; the order of adding additives is optimized through experiments to ensure that they can be evenly dispersed during the subsequent stirring process, and special attention is paid to the distribution uniformity of PVA fiber to ensure the crack resistance and toughness of the slurry;
[0137] S44. After adding PVA fiber, PC-1051 water reducing agent and defoaming agent, restart the auger or elevator to continue conveying the remaining 30% dry powder mixture to the mixing bin;
[0138] S45, after all the dry powder mixture is delivered, the stirring device in the stirring bin is started to fully mix all the components to form a homogeneous slurry;
[0139] S46. After the stirring is completed, the slurry is immediately tested. The test items include the fluidity, viscosity and uniformity of the slurry. According to the test results, if it is found that it does not meet the requirements, the stirring parameters need to be adjusted and the stirring should be repeated until the slurry reaches the expected standards.
[0140] In this implementation, S5 includes the following steps:
[0141] S51, start the mixer and the flying knife to preliminarily mix the materials prepared in claim 6. At this time, the initial speed v of the mixer is s (0) and the initial cutting frequency f of the flying cutter c (0) Set as base value v base and f base; S52, in the primary stirring stage, the multi-level adaptive dispersion algorithm is applied to monitor the viscosity η(t of the slurry and the distribution density ρ of the PVA fiber in real time PVA (t), stirring speed v s (t) and cutting frequency f c (t) Dynamic adjustment is performed according to the following formula:
[0142]
[0143] Where η(t) represents the slurry viscosity at time t; ρ PVA (t) represents the distribution density of PVA fibers at time t; Ψ and Θ are adjustment coefficients;
[0144] S53, in the mid-term stirring stage, the multi-level adaptive dispersion algorithm gradually increases the stirring speed v according to the increase in slurry viscosity and the uniformity of fiber distribution. s (t) and cutting frequency f c (t) to further optimize the dispersion of PVA fibers:
[0145]
[0146] Among them, v opt and f opt is the optimal stirring speed and cutting frequency in the mid-term stage; Ψ and Θ are the adjustment coefficients; η max and ρ PVA,max are the maximum allowable viscosity of the slurry and the maximum allowable fiber distribution density;
[0147] S54. In the later stage of stirring, the multi-level adaptive dispersion algorithm adjusts the stirring speed and the cutting frequency to the final optimized state. The adjustment formula of the stirring speed and the cutting frequency is:
[0148]
[0149] Among them, v final and f final is the final stirring speed and cutting frequency in the later stage; Ψ and Θ are the adjustment coefficients; η target and ρ PVA,target They are the final target values of slurry viscosity and fiber distribution density;
[0150] S55. After the stirring is completed, the slurry is immediately tested, with a focus on the uniformity of the distribution of the PVA fibers and the overall viscosity and fluidity of the slurry. If the test results do not meet the standards, the stirring parameters are adjusted based on the feedback and the stirring is repeated until the expected standards are met.
[0151] Embodiment 1:
[0152] In a new cross-sea bridge project on the southeast coast of my country, the durability and corrosion resistance of the concrete structure became the core problem of engineering design and construction. Due to the high salinity, high humidity and frequent tidal effects in the marine environment, the steel bars in the concrete are easily corroded by chloride ions, leading to steel corrosion, which in turn causes cracking and spalling of the concrete structure. In this environment, traditional grouting mortar often fails to provide long-term and effective protection, especially in key stress-bearing parts such as bridge foundations. The defects of traditional materials may cause serious structural problems, affecting the safety and service life of the bridge.
[0153] In order to solve this problem, the construction team decided to use the rust-resistant high-strength special grouting mortar of the present invention. This mortar not only has excellent mechanical properties, but also significantly enhances the corrosion resistance of the material through innovative formula and preparation process. Its core technologies include adaptive hierarchical reaction control algorithm and multi-level adaptive dispersion algorithm, which ensure the accuracy of material ratio and uniformity of slurry, thereby maximizing the life of reinforced concrete structure.
[0154] In the infrastructure construction of the cross-sea bridge project, the construction team first optimized the ratio of the rust-resistant high-strength special grouting mortar of the present invention. According to the climatic conditions and marine environmental influences of the project site, P.O52.5 ordinary Portland cement, silica fume, fly ash micro-bead powder, mineral powder and quartz sand were selected as the main raw materials. Multiple experiments were carried out through the adaptive hierarchical reaction control algorithm to determine the optimal ratio of the materials, including 425 parts of cement, 40 parts of silica fume, 90 parts of fly ash micro-bead powder, 110 parts of mineral powder, and 460 parts of quartz sand.
[0155] After determining the best ratio, the construction team weighed each raw material in proportion and added them to the mixing equipment in turn. A multi-level adaptive dispersion algorithm is used to control the mixing process to ensure the uniform distribution of additives such as PVA fibers in the slurry. During the mixing process, the viscosity and fiber distribution density of the slurry are monitored in real time, and the mixing parameters are dynamically adjusted according to the actual situation to ensure that the slurry has optimal fluidity and uniformity. After the mixing is completed, the team uses the slurry for grouting construction of the bridge foundation, and tests the physical properties of the slurry many times during the construction process, including compressive strength, fluidity, chloride ion permeability and other indicators to ensure that each batch of mortar meets the design requirements.
[0156] Data proves beneficial effects:
[0157] At different time points after the completion of the bridge foundation construction, the construction team conducted detailed inspections of the cured concrete structure and compared its performance with that of the control area using traditional grouting mortar. The inspection indicators included compressive strength, resistance to chloride ion penetration, and steel bar corrosion rate.
[0158] Table 1 Compressive strength and chloride ion penetration resistance test
[0159]
[0160]
[0161] Table 2 Analysis of steel bar corrosion
[0162] Detection cycle Steel bar corrosion rate (%) Traditional Grouting Mortar Rust-resistant high-strength special grouting mortar 90 days Corrosion rate 8 0.8 180 days Corrosion rate 12.5 1.5 365 days Corrosion rate 15 2.2 540 days Corrosion rate 17.5 2.8 720 days Corrosion rate 20 3.5
[0163] It can be seen from the above test data that the rust-resistant high-strength special grouting mortar of the present invention has shown significant advantages in coastal bridge foundation projects. In terms of compressive strength and resistance to chloride ion penetration, the rust-resistant high-strength special grouting mortar exhibits higher strength and lower chloride ion penetration depth, ensuring the long-term durability of the bridge structure. In addition, the corrosion rate of steel bars exposed to harsh environments for a long time is also much better than that of traditional grouting mortars, indicating that the grouting mortar of the present invention has excellent corrosion resistance. These data prove that the rust-resistant high-strength special grouting mortar of the present invention provides a more reliable and economical solution for infrastructure construction in coastal high-corrosion environments.
[0164] The above description is only a preferred specific implementation manner of the present invention, but the protection scope of the present invention is not limited thereto. Any technician familiar with the technical field can make equivalent replacements or changes according to the technical scheme and inventive concept of the present invention within the technical scope disclosed by the present invention, which should be covered by the protection scope of the present invention.
Claims
1. A rust-resistant high-strength special grouting mortar and a preparation method thereof, characterized in that: The grouting mortar is prepared from the following raw materials in parts by weight: PO52.5 ordinary Portland cement 400-450 parts; silica fume 25-55 parts; fly ash microbead powder 50-100 parts; 800 mesh mineral powder 75-125 parts; 10-120 mesh quartz sand 425-475 parts; PVA fiber 0.3-0.7 parts; PC-1051 water reducer 1.5-3.5 parts; defoaming agent 0.3-0.8 parts.
2. A rust-resistant high-strength special grouting mortar and a preparation method thereof, characterized in that: The steps include: S1. Weigh the PO52.5 ordinary Portland cement, silica fume, fly ash microbead powder, mineral powder, and quartz sand prepared in claim 1, conduct multiple experiments using an adaptive hierarchical reaction control algorithm, generate multiple ingredient combinations, and record relevant experimental data; S2. Based on the experimental data obtained in S1, the optimization algorithm is used to evaluate the performance of each ingredient combination, select the ingredient combination with the best performance, and determine the final optimal ingredient ratio; S3, weighing PO52.5 ordinary Portland cement, silica fume, fly ash microbead powder, mineral powder and quartz sand according to the determined optimal proportion of ingredients, and mixing these components evenly to prepare a dry powder mixture; S4. The dry powder mixture is conveyed to the mixing bin by means of an auger or an elevator. When the conveying reaches 70%, the conveying is stopped, and PVA fiber, PC-1051 water reducing agent and defoaming agent are added. The remaining dry powder mixture is conveyed to the mixing bin. S5, starting the mixer and the flying knife, using a multi-level adaptive dispersion algorithm to regulate the distribution of the PVA fibers, and completing uniform stirring of the slurry; S6. After the stirring is completed, the slurry is tested and the physical and chemical properties are recorded; S7. Based on the test results, use the slurry that meets the requirements for grouting construction and follow the prescribed steps.
3. A rust-resistant high-strength special grouting mortar and a preparation method thereof according to claim 2, characterized in that: The S1 comprises the following steps: S11. Weigh the PO52.5 ordinary Portland cement, silica fume, fly ash microbead powder, mineral powder, and quartz sand prepared in claim 1, and record the mass M of each material respectively. i , where i = 1, 2, 3, 4, 5 correspond to cement, silica fume, fly ash microbead powder, mineral powder, quartz sand, and particle size d i , and the specific surface area S i , for the reaction rate R i (t) Calculation and optimization of material ratio; S12, using the adaptive hierarchical reaction control algorithm, through multiple experiments to determine the hydration reaction rate R of each material i (t) and the degree of reaction E i (t) to generate multiple ingredient combinations and record related data: Among them, R i (t) represents material M i The hydration reaction rate at time t; A i is the material's reactive constant force; S i is the specific surface area of the material; d i is the average particle size of the material; n is the particle size influencing factor; θ(t′) is the thermodynamic reaction angle of the material at time t′; is the time derivative of the thermodynamic reaction angle; δ is the thermodynamic nonlinear characteristic index; E a is the activation energy of the material; γ is the humidity correction coefficient; H is the ambient humidity; R is the gas constant; T is the reaction temperature; m is the nonlinear index of humidity influence; S13, material M i According to particle size d i Divided into different levelsG j , in order to more accurately calculate the reaction rate R at each level i,j (t) and the degree of reaction E i,j (t), the reaction rate R of the material i,j (t) is calculated by the following formula: Among them, R i,j (t) represents the jth level material M i,j The hydration reaction rate at time t; A i,j is the reactivity constant of the j-th level material; S i,j is the specific surface area of the jth level material; d i,j is the particle size of the jth level material; θ j (t) is the thermodynamic reaction angle of the j-th level material; δ j E is the thermodynamic nonlinear characteristic index of the j-th level material; a,j is the activation energy of the jth level material; m j is the nonlinear index of humidity effect; S14. At each grading stage G i After the end, based on the experimental data of the previous level, adjust the addition ratio P of the next level of materials i,j (t) and sequence S i,j (t), in order to optimize the subsequent reaction process, the addition ratio of the material P i,j (t+1) is determined by the following formula: Where, Pi,j(t) represents the addition ratio of the j-th level material at time t; Ei,j(t′) represents the reaction degree of the j-th level material at time t′; It represents the cumulative sum of the reaction rate and reaction extent of all levels of materials at time t; S15. After multiple rounds of experiments, calculate the global reaction effect of each level of material I total , integrate all experimental data, evaluate the comprehensive influence of different proportions on mortar performance, and the global reaction effect I total : Among them, I total Represents the comprehensive response performance of all materials during the entire experiment; σ i,j Contribution of material to compressive strength at level j; S16. Determine the final optimal material ratio P by optimizing the objective function optimal : Among them, P optimal Indicates the optimal material ratio finally determined.
4. The rust-resistant high-strength special grouting mortar and its preparation method according to claim 2, characterized in that: The S2 comprises the following steps: S21. According to the experimental data in claim 3, extract the hydration reaction rate Ri(t), reaction degree E of each ingredient combination i (t) and compressive strength σ i , taking these data as input, we prepare for further optimization analysis; S22, use weighted optimization algorithm to make preliminary evaluation on each ingredient combination, and the comprehensive performance index C i (t) is calculated by the following formula: Among them, C i (t) is the comprehensive performance index of ingredient combination i at time t; α, β, is the weighted coefficient of the optimization algorithm; Ri(t) is the material M i The hydration reaction rate at time t; E i (t) is the material M i The degree of reaction; i For material M i Compressive strength; S23. After the initial evaluation, the adaptive genetic algorithm is used to further optimize the ingredient combination and define the fitness function F(C i ) to evaluate the fitness of each combination, and the fitness function is based on the comprehensive performance index C i (t) Calculate: Among them, F(C i ) is the fitness value of ingredient combination i; max(C i (t)) is the highest comprehensive performance index among all ingredient combinations; S24. In the adaptive genetic algorithm, crossover and mutation operations are used to generate new ingredient combinations P new (t); In each round, the crossover operation is performed using the following formula: P new (t)=λ·P parent1 (t)+(1-λ)·P parent2 (t); Among them, P new (t) is the ratio of the newly generated ingredient combination at time t; P parent1 (t) and P parent2 (t) is the selected parent ingredient combination; λ is the crossover factor, which controls the similarity between the new combination and the parent, and its value is between 0 and 1; S25, the mutation operation adjusts the individual parameters of the newly generated combination according to the following formula: P mutated (t)=P new (t)+∈·N(0,1); Among them, P mutated (t) is the ratio of the mutated ingredient combination at time t; ∈ is the mutation intensity; N(0, 1) is a random variable that obeys the normal distribution; S26. After multiple rounds of crossover and mutation operations, calculate the comprehensive performance index C of the new ingredient combination generated in each round new (t), and recalculate the fitness value F(C new ), and finally select the ingredient combination with the highest fitness as the optimal ingredient ratio after optimization; S27, the final optimized ingredient ratio P optimal Used in the next experiment or actual production.
5. The rust-resistant high-strength special grouting mortar and its preparation method according to claim 2, characterized in that: The S3 comprises the following steps: S31, according to the best proportion of ingredients P determined in claim 4 optimal , weigh PO52.5 ordinary Portland cement M1, silica fume M2, fly ash microbead powder M3, mineral powder M4 and quartz sand M5, the mass of each material is weighed according to the optimal ratio determined in claim 4; S32. After weighing, add PO52.5 ordinary Portland cement M1 to the dry powder mixer first, and then add silica fume M2, fly ash microbead powder M3, mineral powder M4 and quartz sand M5 in sequence; the order of addition depends on the physical properties of the materials; S33. During the mixing process, the speed and time of the mixer are controlled to ensure that all materials are fully mixed and uniformly formed into a homogeneous dry powder mixture. The speed v and mixing time tm of the mixer are determined by the results of the optimization algorithm to avoid stratification and aggregation of materials. S34, after the mixing is completed, the uniformity of the mixture is detected, and the particle size distribution and specific surface area of the mixture are respectively detected using a particle size analyzer and a specific surface area measuring instrument; S35. According to the test results, if it is found that the uniformity of the mixture does not meet the expected standard, adjust the speed and time of the mixer, and re-mix until the uniformity of the mixture meets the requirements. Re-testing is required after each adjustment; S36. Package the final dry powder mixture and mark it with information such as material ratio, mixing time and mixer parameters to facilitate subsequent construction and quality control.
6. The rust-resistant high-strength special grouting mortar and its preparation method according to claim 2, characterized in that: The S4 comprises the following steps: S41. Use an auger or an elevator to gradually convey the dry powder mixture prepared in claim 5 to a mixing bin. During the conveying process, control the conveying rate and conveying amount so that the dry powder mixture enters the mixing bin evenly to avoid local accumulation or uneven distribution in the mixing bin. S42, when the dry powder mixture is conveyed to 70% of the total amount of the mixing bin, the conveying is suspended; S43, after pausing the conveying, add PVA fiber, PC-1051 water reducing agent and defoaming agent in sequence; the order of adding additives is optimized through experiments to ensure that they can be evenly dispersed during the subsequent stirring process, and special attention is paid to the distribution uniformity of PVA fiber to ensure the crack resistance and toughness of the slurry; S44. After adding PVA fiber, PC-1051 water reducing agent and defoaming agent, restart the auger or elevator to continue conveying the remaining 30% dry powder mixture to the mixing bin; S45, after all the dry powder mixture is delivered, the stirring device in the stirring bin is started to fully mix all the components to form a homogeneous slurry; S46. After the stirring is completed, the slurry is immediately tested. The test items include the fluidity, viscosity and uniformity of the slurry. According to the test results, if it is found that it does not meet the requirements, the stirring parameters need to be adjusted and the stirring should be repeated until the slurry reaches the expected standards.
7. The rust-resistant high-strength special grouting mortar and its preparation method according to claim 2, characterized in that: The S5 The following steps are involved: S51, start the mixer and the flying knife to preliminarily mix the materials prepared in claim 6. At this time, the initial speed v of the mixer is s (0) and the initial cutting frequency f of the flying cutter c (0) Set as base value v base and f base ; S52. In the primary stirring stage, a multi-level adaptive dispersion algorithm is applied to monitor the viscosity η(t) of the slurry and the distribution density ρ of the PVA fibers in real time. PVA (t), stirring speed v s (t) and cutting frequency f c (t) Dynamic adjustment is performed according to the following formula: Where η(t) represents the slurry viscosity at time t; ρ PVA (t) represents the distribution density of PVA fibers at time t; Ψ and Θ are adjustment coefficients; S53, in the mid-term stirring stage, the multi-level adaptive dispersion algorithm gradually increases the stirring speed v according to the increase in slurry viscosity and the uniformity of fiber distribution. s (t) and cutting frequency f c (t) to further optimize the dispersion of PVA fibers: Among them, v opt and f opt is the optimal stirring speed and cutting frequency in the mid-term stage; Ψ and Θ are the adjustment coefficients; η max and ρ PVA,max are the maximum allowable viscosity of the slurry and the maximum allowable fiber distribution density; S54. In the later stage of stirring, the multi-level adaptive dispersion algorithm adjusts the stirring speed and the cutting frequency to the final optimized state. The adjustment formula of the stirring speed and the cutting frequency is: Among them, v final and f final is the final stirring speed and cutting frequency in the later stage; Ψ and Θ are the adjustment coefficients; η target and ρ PVA,target They are the final target values of slurry viscosity and fiber distribution density; S55. After the stirring is completed, the slurry is immediately tested, with a focus on the uniformity of the distribution of the PVA fibers and the overall viscosity and fluidity of the slurry. If the test results do not meet the standards, the stirring parameters are adjusted based on the feedback and the stirring is repeated until the expected standards are met.