Nano SiO2 modified basalt fiber material and preparation method thereof

By laying polyamino acid composite fibers and porous silicon particles on the surface of the basalt fiber base material and performing hot pressing composite, the problem of insufficient toughness of nano-silica modified basalt fiber materials is solved, and the toughness and service life of the material are improved.

CN119080535AActive Publication Date: 2024-12-06四川文理学院 +2

Patent Information

Application Number
CN202411211512.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06
Estimated Expiration
2044-08-30

AI Technical Summary

Technical Problem

Nanosilicon dioxide modified basalt fiber materials have problems of poor toughness or poor toughness stability during long-term use, which has affected their scope of application and further development.

Method used

Using the interlayer toughening material method, polyamino acid composite fibers and porous silicon particles are laid on the surface of the basalt fiber base material, combined with epoxy resin and curing agent, and hot pressing composite is carried out to form nano-SiO2 modified basalt fiber material, which improves the Its fracture toughness and impact resistance.

Benefits of technology

The toughness and strength of basalt fiber materials are significantly improved, the problem of toughness instability is reduced, and the performance stability of the material under high temperature and cyclic treatment is enhanced.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention relates to the technical field of basalt fiber, and discloses a nano SiO2 modified basalt fiber material and a preparation method thereof, the nano SiO2 modified basalt fiber material comprises SiO2-coated basalt fiber, polyamino acid composite fiber and porous silicon particles; the polyamino acid composite fiber comprises a regular molecular chain formed by connecting same amino acids through peptide bonds and an irregular molecular chain formed by connecting different amino acids through peptide bonds. The polyamino acid composite fibers are additionally arranged between basalt fiber base material layers, the polyamino acid composite fibers contain regular molecular chains and irregular molecular chains at the same time, so that the fiber material can be endowed with good toughness and strength, and the polyamino acid composite fibers are combined between the basalt fiber base materials through the porous structure particles; the problems that the toughness of the existing basalt fiber material is unstable and reduced in the using process can be solved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of basalt fibers, and in particular to a nano-SiO2 modified basalt fiber material and a preparation method thereof. Background Art

[0002] Basalt fiber is a continuous fiber drawn from natural basalt stone. It not only has high strength, but also has many excellent properties such as electrical insulation, corrosion resistance, and high temperature resistance. It is listed as one of the four major fibers that my country focuses on developing. It is widely used in fiber-reinforced composite materials, friction materials, shipbuilding materials, thermal insulation materials, the automotive industry, high-temperature filter fabrics, and protection fields.

[0003] Modifying the surface of basalt fiber with nano-silicon dioxide is an effective way to improve the performance of basalt fiber materials. For example, the patent with publication number CN117228974A proposes a method for grafting and modifying basalt fiber, wherein basalt fiber is etched to obtain etched basalt fiber; a graft suspension is mixed with a silane coupling agent solution to obtain a modified solution; the grafted material in the graft suspension includes nano-attapulgite or nano-silicon dioxide; the obtained etched basalt fiber is mixed with the obtained modified solution and then subjected to a grafting reaction to obtain a grafted basalt fiber. Introducing materials such as nano-silicon dioxide on the surface of basalt fiber can increase the roughness and effective contact area of ​​the fiber surface, thereby improving the compatibility or wettability of basalt fiber with other materials.

[0004] However, the existing basalt fiber materials modified by nano-silica, such as the above, have the problem of poor toughness or poor toughness stability during use, which greatly affects the application scope and further development of basalt fiber. Summary of the invention

[0005] The technical problems to be solved by the present invention are:

[0006] At present, using nano-silicon dioxide to modify the surface of basalt fiber is a common way to improve the performance of basalt fiber materials. However, the basalt fiber products obtained by modifying the surface of basalt fiber with nano-silicon dioxide have problems of poor toughness or poor toughness stability during long-term use, which greatly affects the scope of application and further development of basalt fiber.

[0007] The technical solution adopted by the present invention is:

[0008] The present invention provides a nano-SiO2 modified basalt fiber material, comprising SiO2@basalt fiber, polyamino acid composite fiber and porous silicon particles;

[0009] The polyamino acid composite fiber contains regular molecular chains formed by connecting the same amino acids and irregular molecular chains formed by connecting different amino acids.

[0010] Preferably, the amino acids include one or more of glycine, alanine, serine and proline.

[0011] Preferably, the porous silicon particles include one or more of silicon carbide, silicon nitride, silicon dioxide, and POSS.

[0012] Preferably, the particle size of the porous silicon particles is 30-75 nm, and the porosity of the porous silicon particles is 40-60%.

[0013] The present invention also provides a method for preparing the above-mentioned nano-SiO2 modified basalt fiber material, comprising the following steps:

[0014] S1 Preparation of interlayer toughening material:

[0015] The polyamino acid composite fiber is mixed with porous silicon particles, epoxy resin and curing agent, and heated and impregnated to obtain an interlayer toughening material;

[0016] S2 prepares the nano-SiO2 modified basalt fiber material:

[0017] The interlayer toughening material is laid on the surface of the basalt fiber base material while it is hot, and hot-pressed and composited to obtain the nano-SiO2 modified basalt fiber material.

[0018] Preferably, in step S1, the method for preparing the polyamino acid composite fiber comprises the following steps:

[0019] Polyethylene glycol and isocyanate are mixed, a catalyst is added, and a prepolymer is obtained by reaction; polyamino acid ester and an organic solvent are added to the prepolymer, mixed and reacted, a precipitate is precipitated, and spinning is performed to obtain the polyamino acid composite fiber.

[0020] Preferably, in step S1, the heating and dipping temperature is 100-120°C.

[0021] Preferably, in step S2, the method for preparing the basalt fiber base material comprises the following steps:

[0022] The basalt fiber is placed in an acidic environment for surface activation treatment and hydrochloric acid etching; the etched basalt fiber is placed in a mesoporous silica composite liquid for heating and impregnation treatment to obtain a basalt fiber base material modified by silica.

[0023] Preferably, the mesoporous silica composite liquid comprises nano-silica, a surfactant, an organic silicon solvent and deionized water.

[0024] Preferably, when preparing the basalt fiber base material, the heating and impregnation temperature is 30-50° C. and the treatment time is 1-2 hours.

[0025] The beneficial effects of the present invention are as follows:

[0026] The present invention adopts the interlayer toughening method to improve the fracture toughness and impact resistance of basalt fiber composite materials. By adding polyamino acid composite fibers between the layers of basalt fiber base materials, since the polyamino acid composite fibers contain both regular molecular chains and irregular molecular chains, the fiber material can be given good toughness and strength, and the polyamino acid composite fibers are combined with the basalt fiber base materials through porous structure particles, which can improve the problem of unstable and reduced toughness of existing basalt fiber materials during use. DETAILED DESCRIPTION

[0027] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0028] The invention provides a nano-SiO2 modified basalt fiber material, comprising SiO2@basalt fiber, polyamino acid composite fiber and porous silicon particles.

[0029] In the present invention, SiO2@basalt fiber refers to basalt fiber obtained by surface modification with silicon dioxide.

[0030] In the present invention, the polyamino acid composite fiber contains both a regular molecular chain structure formed by connecting the same amino acids and an irregular molecular chain structure formed by connecting different amino acids, which can give the fiber material good toughness and strength; specifically, the multiple amino acids include but are not limited to one or more of glycine, alanine, serine and proline.

[0031] In the present invention, the porous silicon particles include but are not limited to one or more of silicon carbide, silicon nitride, silicon dioxide, POSS, etc., and the particle size of the porous silicon particles is 30-75nm, and the pore volume of the porous silicon particles is 40-60%.

[0032] The present invention also provides a method for preparing the above-mentioned nano-SiO2 modified basalt fiber material, comprising the following steps:

[0033] (1) Preparation of basalt fiber base material

[0034] The basalt fiber is placed in an acidic environment for surface activation and hydrochloric acid etching. The etched basalt fiber is then placed in a mesoporous silica composite liquid, heated to 30-50°C, and immersed for 1-2 hours to obtain a basalt fiber base material with nano-silica attached to the surface.

[0035] The mesoporous silica composite liquid includes nano-silica, surfactant, organic silicon solvent and deionized water, etc., and is mixed by stirring; the particle size of the nano-silica is about 5-30nm.

[0036] (2) Preparation of interlayer toughening materials

[0037] Polyethylene glycol and isocyanate are mixed, a catalyst is added, and a prepolymer is obtained by reaction; a polyamino acid ester in a β-folded state and an organic solvent are added to the prepolymer, and the mixture is reacted to form a polymerized amino acid having regular molecular segments containing some repeating units and molecular segments having a spatially irregular structure, and a precipitate is precipitated, and then spinning is performed to obtain a polyamino acid composite fiber;

[0038] The prepared polyamino acid composite fiber is mixed and impregnated with porous silicon particles, epoxy resin and curing agent, and heated to 100-120° C. for hot-melt compounding to obtain an interlayer toughening material.

[0039] Among them, the polyamino acid composite fiber is a kind of spider silk-like spinning fiber, so spider silk fiber can also be directly used to replace the polyamino acid composite fiber.

[0040] (3) Preparation of nano-SiO2 modified basalt fiber materials

[0041] The interlayer toughening material is laid on the surface of the basalt fiber base material while hot to fully cover and infiltrate it. During this operation, the temperature of the interlayer toughening material is maintained above 60°C. After hot pressing and compounding, a nano-SiO2 modified basalt fiber material with a toughening interlayer is obtained.

[0042] Example 1

[0043] Step 1: Take 2.5 parts by mass of nano-silica with a particle size of 20±10 nm, mix it with 0.3 parts by mass of hexadecyltrimethylammonium chloride, 0.1 parts by mass of potassium persulfate, 2 parts by mass of dimethylsiloxane and 2 parts by mass of deionized water, and stir at 200 r / min for 5 minutes to obtain a mesoporous silica composite liquid.

[0044] Step 2: Take basalt fiber, place it in a mixed solution containing equal masses of sulfuric acid and hydrogen peroxide to perform surface activation treatment, and then etch its surface with hydrochloric acid to form a basalt fiber with a high specific surface area; place the basalt fiber obtained by the above treatment in a mesoporous silica composite solution, heat it to 40±3°C, and immerse it for 1.5 hours to obtain a basalt fiber base material with nano-silica connected to the surface.

[0045] Step 3: Take equimolar masses of polyethylene glycol (molecular weight is about 1850) and diisocyanate, mix them, add dibutyltin dilaurate, and react to obtain a prepolymer; then add poly-β-amino acid ester and dimethylformamide to the prepolymer, mix and react, then add methanol to precipitate, and prepare polyamino acid composite fibers by dry spinning.

[0046] Step 4: Take 56.2wt% of polyamino acid composite fiber and 40.5wt% of vinyl POSS, add glycidyl epoxy resin and aromatic amine curing agent, mix and impregnate, heat to 108±2°C for hot melt compounding, and obtain an interlayer toughening material.

[0047] Step 5: Lay the interlayer toughening material on the surface of the basalt fiber base material while it is hot, keep the interlayer toughening material at 80±10°C to allow it to be fully covered and infiltrated, and perform hot pressing and compounding to produce a nano-SiO2 modified basalt fiber material containing a toughening interlayer.

[0048] The above product was tested at room temperature. At a tensile rate of 20 mm / min, the tensile strength was 893 MPa, the elastic modulus was 102 Gpa, and the toughness was 304 MJ / m 3 After a cycle of heating at 100°C and cooling at 25°C, its toughness was measured to decrease by 4.2%.

[0049] Example 2

[0050] Step 1: Take 2.5 parts by mass of nano-silica with a particle size of 20±10 nm, mix it with 0.3 parts by mass of hexadecyltrimethylammonium chloride, 0.1 parts by mass of potassium persulfate, 2 parts by mass of dimethylsiloxane and 2 parts by mass of deionized water, and stir at 200 r / min for 5 minutes to obtain a mesoporous silica composite liquid.

[0051] Step 2: Take basalt fiber, place it in a mixed solution containing equal masses of sulfuric acid and hydrogen peroxide to perform surface activation treatment, and then etch its surface with hydrochloric acid to form a basalt fiber with a high specific surface area; place the basalt fiber obtained by the above treatment in a mesoporous silica composite solution, heat it to 40±3°C, and immerse it for 1.5 hours to obtain a basalt fiber base material with nano-silica connected to the surface.

[0052] Step 3: Take equimolar masses of polyethylene glycol (molecular weight is about 1850) and diisocyanate, mix them, add dibutyltin dilaurate, and react to obtain a prepolymer; then add poly-β-amino acid ester and dimethylformamide to the prepolymer, mix and react, then add methanol to precipitate, and prepare polyamino acid composite fibers by dry spinning.

[0053] Step 4: Take another 42wt% of polyamino acid composite fiber and 55wt% of vinyl POSS, add glycidyl epoxy resin and aromatic amine curing agent, mix and impregnate, heat to 108±2°C for hot melt compounding, and obtain an interlayer toughening material.

[0054] Step 5: Lay the interlayer toughening material on the surface of the basalt fiber base material while it is hot, keep the interlayer toughening material at 80±10°C to allow it to be fully covered and infiltrated, and perform hot pressing and compounding to produce a nano-SiO2 modified basalt fiber material containing a toughening interlayer.

[0055] The above product was tested at room temperature. At a tensile rate of 20 mm / min, the tensile strength was 871 MPa, the elastic modulus was 104 Gpa, and the toughness was 301 MJ / m 3 After a cycle of heating at 100°C and cooling at 25°C, its toughness was measured to decrease by 4.6%.

[0056] Example 3

[0057] Step 1: Take 2.5 parts by mass of nano-silica with a particle size of 20±10 nm, mix it with 0.3 parts by mass of hexadecyltrimethylammonium chloride, 0.1 parts by mass of potassium persulfate, 2 parts by mass of dimethylsiloxane and 2 parts by mass of deionized water, and stir at 200 r / min for 5 minutes to obtain a mesoporous silica composite liquid.

[0058] Step 2: Take basalt fiber, place it in a mixed solution containing equal masses of sulfuric acid and hydrogen peroxide to perform surface activation treatment, and then etch its surface with hydrochloric acid to form a basalt fiber with a high specific surface area; place the basalt fiber obtained by the above treatment in a mesoporous silica composite solution, heat it to 40±3°C, and immerse it for 1.5 hours to obtain a basalt fiber base material with nano-silica connected to the surface.

[0059] Step 3: Take equimolar masses of polyethylene glycol (molecular weight is about 1850) and diisocyanate, mix them, add dibutyltin dilaurate, and react to obtain a prepolymer; then add poly-β-amino acid ester and dimethylformamide to the prepolymer, mix and react, then add methanol to precipitate, and prepare polyamino acid composite fibers by dry spinning.

[0060] Step 4: Take another 60.3wt% of polyamino acid composite fiber and 35.8wt% of vinyl POSS, add glycidyl epoxy resin and aromatic amine curing agent, mix and impregnate, heat to 108±2°C for hot melt compounding, and obtain an interlayer toughening material.

[0061] Step 5: Lay the interlayer toughening material on the surface of the basalt fiber base material while it is hot, keep the interlayer toughening material at 80±10°C to allow it to be fully covered and infiltrated, and perform hot pressing and compounding to produce a nano-SiO2 modified basalt fiber material containing a toughening interlayer.

[0062] The above product was tested at room temperature. At a tensile rate of 20 mm / min, the tensile strength was 884 MPa, the elastic modulus was 104 Gpa, and the toughness was 303 MJ / m 3 After a cycle of heating at 100°C and cooling at 25°C, its toughness was measured to decrease by 4.4%.

[0063] Example 4

[0064] Step 1: Take 2.5 parts by mass of nano-silica with a particle size of 20±10 nm, mix it with 0.3 parts by mass of hexadecyltrimethylammonium chloride, 0.1 parts by mass of potassium persulfate, 2 parts by mass of dimethylsiloxane and 2 parts by mass of deionized water, and stir at 200 r / min for 5 minutes to obtain a mesoporous silica composite liquid.

[0065] Step 2: Take basalt fiber, place it in a mixed solution containing equal masses of sulfuric acid and hydrogen peroxide to perform surface activation treatment, and then etch its surface with hydrochloric acid to form a basalt fiber with a high specific surface area; place the basalt fiber obtained by the above treatment in a mesoporous silica composite solution, heat it to 40±3°C, and immerse it for 1.5 hours to obtain a basalt fiber base material with nano-silica connected to the surface.

[0066] Step 3: Take equimolar masses of polyethylene glycol (molecular weight is about 1850) and diisocyanate, mix them, add dibutyltin dilaurate, and react to obtain a prepolymer; then add poly-β-amino acid ester and dimethylformamide to the prepolymer, mix and react, then add methanol to precipitate, and prepare polyamino acid composite fibers by dry spinning.

[0067] Step 4: Take another 23.7wt% of polyamino acid composite fiber and 25.0wt% of vinyl POSS, add glycidyl epoxy resin and aromatic amine curing agent, add water to mix and impregnate, heat to 108±2°C for hot melt compounding, and obtain an interlayer toughening material.

[0068] Step 5: Lay the interlayer toughening material on the surface of the basalt fiber base material while it is hot, keep the interlayer toughening material at 80±10°C to allow it to be fully covered and infiltrated, and perform hot pressing and compounding to produce a nano-SiO2 modified basalt fiber material containing a toughening interlayer.

[0069] The above product was tested at room temperature. At a tensile rate of 20 mm / min, the tensile strength was 847 MPa, the elastic modulus was 105 Gpa, and the toughness was 290 MJ / m 3 After a cycle of heating at 100°C and cooling at 25°C, its toughness was measured to decrease by 8.6%.

[0070] Example 5

[0071] Step 1: Take 2.5 parts by mass of nano-silica with a particle size of 20±10 nm, mix it with 0.3 parts by mass of hexadecyltrimethylammonium chloride, 0.1 parts by mass of potassium persulfate, 2 parts by mass of dimethylsiloxane and 2 parts by mass of deionized water, and stir at 200 r / min for 5 minutes to obtain a mesoporous silica composite liquid.

[0072] Step 2: Take basalt fiber, place it in a mixed solution containing equal masses of sulfuric acid and hydrogen peroxide to perform surface activation treatment, and then etch its surface with hydrochloric acid to form a basalt fiber with a high specific surface area; place the basalt fiber obtained by the above treatment in a mesoporous silica composite solution, heat it to 40±3°C, and immerse it for 1.5 hours to obtain a basalt fiber base material with nano-silica connected to the surface.

[0073] Step 3: Take equimolar masses of polyethylene glycol (molecular weight of about 1850) and diisocyanate, mix them, add dibutyltin dilaurate, and react to obtain a prepolymer; then add spider silk fiber to the prepolymer, mix them, and prepare polyamino acid composite fibers by dry spinning.

[0074] Step 4: Take 56.2wt% of polyamino acid composite fiber and 40.5wt% of vinyl POSS, add glycidyl epoxy resin and aromatic amine curing agent, mix and impregnate, heat to 108±2°C for hot melt compounding, and obtain an interlayer toughening material.

[0075] Step 5: Lay the interlayer toughening material on the surface of the basalt fiber base material while it is hot, keep the interlayer toughening material at 80±10°C to allow it to be fully covered and infiltrated, and perform hot pressing and compounding to produce a nano-SiO2 modified basalt fiber material containing a toughening interlayer.

[0076] The above product was tested at room temperature. At a tensile rate of 20 mm / min, the tensile strength was 895 MPa, the elastic modulus was 103 Gpa, and the toughness was 311 MJ / m 3After a cycle of heating at 100°C and cooling at 25°C, its toughness was measured to decrease by 6.4%.

[0077] Comparative Example 1

[0078] Step 1: Take 2.5 parts by mass of nano-silica with a particle size of 20±10 nm, mix it with 0.3 parts by mass of hexadecyltrimethylammonium chloride, 0.1 parts by mass of potassium persulfate, 2 parts by mass of dimethylsiloxane and 2 parts by mass of deionized water, and stir at 200 r / min for 5 minutes to obtain a mesoporous silica composite liquid.

[0079] Step 2: Take basalt fiber, place it in a mixed solution containing equal masses of sulfuric acid and hydrogen peroxide to perform surface activation treatment, and then etch its surface with hydrochloric acid to form a basalt fiber with a high specific surface area; place the basalt fiber obtained by the above treatment in a mesoporous silica composite solution, heat it to 40±3°C, and immerse it for 1.5 hours to obtain a basalt fiber material with nano-silica attached to the surface.

[0080] The above product was tested at room temperature. At a tensile rate of 20 mm / min, the tensile strength was 795 MPa, the elastic modulus was 109 Gpa, and the toughness was 265 MJ / m 3 After a cycle of heating at 100°C and cooling at 25°C, its toughness was measured to decrease by 36.1%.

[0081] Comparative Example 2

[0082] Step 1: Take 2.5 parts by mass of nano-silica with a particle size of 20±10 nm, mix it with 0.3 parts by mass of hexadecyltrimethylammonium chloride, 0.1 parts by mass of potassium persulfate, 2 parts by mass of dimethylsiloxane and 2 parts by mass of deionized water, and stir at 200 r / min for 5 minutes to obtain a mesoporous silica composite liquid.

[0083] Step 2: Take basalt fiber, place it in a mixed solution containing equal masses of sulfuric acid and hydrogen peroxide to perform surface activation treatment, and then etch its surface with hydrochloric acid to form a basalt fiber with a high specific surface area; place the basalt fiber obtained by the above treatment in a mesoporous silica composite solution, heat it to 40±3°C, and immerse it for 1.5 hours to obtain a basalt fiber base material with nano-silica connected to the surface.

[0084] Step 3: Take equimolar masses of polyethylene glycol (molecular weight is about 1850) and diisocyanate, mix them, add dibutyltin dilaurate, and react to obtain a prepolymer; then add poly-β-amino acid ester and dimethylformamide to the prepolymer, mix and react, then add methanol to precipitate, and prepare polyamino acid composite fibers by dry spinning.

[0085] Step 4: Take another 56.2 wt % of polyamino acid composite fiber and glycidyl epoxy resin, add water, mix and impregnate, heat to 108±2° C. for hot-melt compounding, and obtain a toughened slurry.

[0086] Step 5: Lay the toughening slurry on the surface of the basalt fiber base material while it is hot, keep the toughening slurry at 80±10°C to fully cover and infiltrate it, and perform hot pressing and compounding to obtain a basalt fiber material with a multi-layer structure.

[0087] The above product was tested at room temperature. At a tensile rate of 20 mm / min, the tensile strength was 859 MPa, the elastic modulus was 106 Gpa, and the toughness was 298 MJ / m 3 After a cycle of heating at 100°C and cooling at 25°C, its toughness was measured to decrease by 10.3%.

[0088] Comparative Example 3

[0089] Step 1: Take 2.5 parts by mass of nano-silica with a particle size of 20±10 nm, mix it with 0.3 parts by mass of hexadecyltrimethylammonium chloride, 0.1 parts by mass of potassium persulfate, 2 parts by mass of dimethylsiloxane and 2 parts by mass of deionized water, and stir at 200 r / min for 5 minutes to obtain a mesoporous silica composite liquid.

[0090] Step 2: Take basalt fiber, place it in a mixed solution containing equal masses of sulfuric acid and hydrogen peroxide to perform surface activation treatment, and then etch its surface with hydrochloric acid to form a basalt fiber with a high specific surface area; place the basalt fiber obtained by the above treatment in a mesoporous silica composite solution, heat it to 40±3°C, and immerse it for 1.5 hours to obtain a basalt fiber base material with nano-silica connected to the surface.

[0091] Step 3: Take vinyl POSS, glycidyl epoxy resin and aromatic amine curing agent, add water to mix and impregnate, heat to 108±2° C. for hot melt compounding, and obtain a toughened slurry.

[0092] Step 4: Lay the toughening slurry on the surface of the basalt fiber base material while it is hot, keep the toughening slurry at 80±10℃ to fully cover and infiltrate it, and perform hot pressing and compounding to form a basalt fiber material with a multi-layer structure.

[0093] The above product was tested at room temperature. At a tensile rate of 20 mm / min, the tensile strength was 852 MPa, the elastic modulus was 107 Gpa, and the toughness was 295 MJ / m 3 After a cycle of heating at 100°C and cooling at 25°C, its toughness was measured to decrease by 12.1%.

[0094] By comparing the above embodiments and comparative examples, it can be seen that the toughness of the nano-SiO2 modified basalt fiber material in the embodiment is slightly higher than that of the basalt fiber material in the comparative example at room temperature in the initial state; and after multiple treatments of high-temperature heating and low-temperature cooling, the degree of decrease in toughness of the nano-SiO2 modified basalt fiber material in the embodiment is significantly lower than that of the basalt fiber material in the comparative example. Therefore, the above test can illustrate that the nano-SiO2 modified basalt fiber material and the preparation method thereof proposed in the present invention can effectively solve the problem of poor toughness or poor toughness stability of the current silica modified basalt fiber material, that is, effectively improve the performance and service life of the basalt fiber material.

[0095] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. For those skilled in the art, the present invention may have various modifications and variations. Any modification, equivalent replacement, improvement, etc. made within the spirit and principle of the present invention shall be included in the protection scope of the present invention.

Claims

1. A nano-SiO 2 Modified basalt fiber material, It is characterized in that Including SiO 2 @Basalt fiber, polyamino acid composite fiber and porous silicon particles; The polyamino acid composite fiber contains regular molecular chains formed by connecting the same amino acids and irregular molecular chains formed by connecting different amino acids.

2. Nano-SiO according to claim 1 2 Modified basalt fiber material, It is characterized in that The amino acids include one or more of glycine, alanine, serine and proline.

3. Nano-SiO according to claim 1 or 2 2 Modified basalt fiber material, It is characterized in that The porous silicon particles include one or more of silicon carbide, silicon nitride, silicon dioxide, and POSS.

4. Nano-SiO according to claim 3 2 Modified basalt fiber material, It is characterized in that The particle size of the porous silicon particles is 30-75 nm, and the porosity of the porous silicon particles is 40-60%.

5. A nano-SiO according to any one of claims 1 to 4 2 Preparation method of modified basalt fiber material, It is characterized in that The steps include: S1 Preparation of interlayer toughening material: The polyamino acid composite fiber is mixed with porous silicon particles, epoxy resin and curing agent, and heated and impregnated to obtain an interlayer toughening material; S2 Preparation of the Nano-SiO 2 Modified basalt fiber materials: The interlayer toughening material is laid on the surface of the basalt fiber base material while it is hot, and hot-pressed to obtain the nano-SiO 2 Modified basalt fiber material.

6. Nano-SiO according to claim 5 2 Preparation method of modified basalt fiber material, It is characterized in that In step S1, the method for preparing the polyamino acid composite fiber comprises the following steps: Polyethylene glycol and isocyanate are mixed, a catalyst is added, and a prepolymer is obtained by reaction; polyamino acid ester and an organic solvent are added to the prepolymer, mixed and reacted, a precipitate is precipitated, and spinning is performed to obtain the polyamino acid composite fiber.

7. The nano-SiO according to claim 5 2 Preparation method of modified basalt fiber material, It is characterized in that In step S1, the heating and dipping temperature is 100-120°C.

8. The nano-SiO according to claim 5 2 Preparation method of modified basalt fiber material, It is characterized in that In step S2, the method for preparing the basalt fiber base material comprises the following steps: The basalt fiber is placed in an acidic environment for surface activation treatment and hydrochloric acid etching; the etched basalt fiber is placed in a mesoporous silica composite liquid for heating and impregnation treatment to obtain a basalt fiber base material modified by silica.

9. The nano-SiO according to claim 8 2 Preparation method of modified basalt fiber material, It is characterized in that The mesoporous silica composite liquid comprises nano-silicon dioxide, a surfactant, an organic silicon solvent and deionized water.

10. The nano-SiO according to claim 8 2 Preparation method of modified basalt fiber material, It is characterized in that When preparing the basalt fiber base material, the heating and impregnation temperature is 30-50° C. and the treatment time is 1-2 hours.

Citation Information

Patent Citations

  • Preparation method for high-temperature-resistant and fatigue-resistant irradiation-crosslinked polyurethane fibers

    CN105088392A

  • Spider silk-like polymer fiber based on silica porous microspheres and preparation method thereof

    CN109208108A

  • Method for interlayer toughening of carbon fiber prepreg through nano-particle polymer composite nano-fiber membrane

    CN113002024A

  • Production method for preparing interlayer toughened carbon fiber prepreg through one-step method

    CN114181416A

  • Treatment method of polyurethane elastic fiber

    CN116043358A

Cited By

  • Basalt fiber reinforced material for wind power blade and preparation method of basalt fiber reinforced material

    CN121718147A