Diamine, polyamide acid, polyimide, liquid crystal alignment agent and liquid crystal alignment film
The traditional liquid crystal orientation technology is solved by using polyamic acid or polyimide prepared by using diamines with 2,5-diaminoaniline-1,3,4-oxadiazole structure as liquid crystal alignment agent. The problem of insufficient orientation function under irradiation amount has achieved excellent orientation performance and high voltage retention rate of the liquid crystal display element.
Patent Information
- Application Number
- CN202411249658.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-06
- Publication Date
- 2024-12-06
AI Technical Summary
Traditional LCD orientation technology such as friction orientation method has problems such as surface scratches, debris, static electricity and poor alignment in the concave and convex areas in the surface, which cannot meet the needs of modern LCD displays for high-quality displays and high yields, and the linear ultraviolet light is Insufficient orientation function under low irradiation.
Develop a diamine with a 2,5-diaminoaniline-1,3,4-oxadiazole structure, and polyamic acid or polyimide prepared therethrough is used as a liquid crystal alignment agent for preparing liquid crystal alignment films , it is used to achieve excellent orientation of liquid crystal molecules under low ultraviolet irradiation.
The liquid crystal orientation film has good orientation function under low ultraviolet light irradiation, which significantly improves the orientation performance, voltage retention rate, friction resistance and contrast of the liquid crystal display element, and reduces the afterimage phenomenon.
Smart Images

Figure CN119080713A_ABST
Abstract
Description
Technical Field
[0001] The present invention belongs to the technical field of liquid crystal alignment agents, and in particular relates to a diamine, a polyamic acid, a polyimide, a liquid crystal alignment agent and a liquid crystal alignment film. Background Art
[0002] The liquid crystal display element is composed of a transparent substrate with a control electrode, a color film substrate with a regular arrangement of RGB three pigments, and an intermediate layer, wherein the intermediate layer is equipped with a liquid crystal layer. In the liquid crystal display element, the liquid crystal layer between the two substrates is required to be arranged on the liquid crystal orientation film in a certain orientation state. The basic requirements of the liquid crystal orientation film are that it has a good orientation effect on the liquid crystal, a high voltage holding rate, and can release residual charges without residual images.
[0003] As LCD screens have a high cost-effectiveness, they are increasingly used in various industries, and customers have higher and higher requirements for the quality of display images and the yield rate of factory production lines. Therefore, in order to optimize the performance and application effects of liquid crystal materials, it is necessary to use liquid crystal orientation technology to achieve precise control of the arrangement of liquid crystal molecules, thereby achieving the above purpose. Traditional liquid crystal orientation technology uses friction orientation method, which can achieve the orientation of liquid crystal to a certain extent, but it is prone to various problems such as surface scratches, debris, static electricity, and poor orientation of concave and convex parts in the surface, which can no longer meet the existing needs.
[0004] As a method to replace the rubbing alignment, the use of linearly polarized ultraviolet light to irradiate the surface of the liquid crystal alignment film to achieve liquid crystal alignment is developed. The basic principle is that the linearly polarized ultraviolet light has a specific polarization direction. When this light is irradiated to the surface of the liquid crystal alignment film, it will interact with the molecules or structures on the surface of the film, causing the molecules or structures to rearrange or orient in a specific direction, thereby achieving the orientation control of the liquid crystal. In practical applications, the light source of linearly polarized ultraviolet light uses a high-pressure mercury lamp. In order to irradiate more glass substrates within its service life and reduce production costs, the photo-oriented liquid crystal alignment film is required to have an orientation function under low ultraviolet light exposure. Summary of the invention
[0005] The purpose of the present invention is to overcome the above problems existing in the prior art and provide a diamine, a polyamic acid, a polyimide, a liquid crystal orientation agent and a liquid crystal orientation film. The diamine has a structure shown in Formula I. The diamine having the structure shown in Formula I can be used as a raw material for polyamic acid. The prepared polyamic acid is prepared by dehydration and ring closure to obtain polyimide. The prepared polyamic acid or polyimide can be used as a raw material for a liquid crystal orientation agent. The liquid crystal orientation agent is used to prepare a liquid crystal orientation film. The prepared liquid crystal orientation film has good orientation function under low ultraviolet light exposure.
[0006] In order to achieve the above technical objectives and the above technical effects, the present invention is implemented through the following technical solutions:
[0007] The embodiment of the first aspect of the present invention provides a diamine having a structure shown in formula (I):
[0008]
[0009] Wherein, R1 and R2 are independently any one of hydrogen atom, halogen, -CF3, C1-C18 alkyl, -OCH3, -OC2H5, -COOCH3, aromatic compound containing 1-5 benzene rings or compound containing 1-5 heterocyclic rings;
[0010] X1 and X2 are each independently a single bond, -CH2-, -CH2CH2-, -C2H4-, -C(CH3)2-, -CH2O-, -CH2OCH2-, -HNCO-,
[0011] Any of the following:
[0012] m and n are any integers between 0 and 4 respectively.
[0013] Furthermore, m and n are any integers between 1 and 2 respectively.
[0014] Furthermore, the diamine is selected from any one or more combinations of compounds represented by the following formulae (1-1) to (1-22);
[0015]
[0016]
[0017]
[0018] The embodiment of the second aspect of the present invention provides a polyamic acid, which is prepared by mixing a diamine compound, a tetracarboxylic acid derivative and a solvent, and then reacting the mixture to obtain a polyamic acid solution comprising the polyamic acid;
[0019] The diamine compound includes the diamine described in the embodiment of the first aspect of the present invention.
[0020] Further, the diamine compound also includes diamine B;
[0021] The diamine B is 1,2-diaminoethane, 1,3-diaminopropane, 1,4-diaminobutane, 1,6-diaminohexane, p-phenylenediamine, 1,5-naphthalenediamine, 1,8-diaminonaphthalene, 4,4'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylamine, 4,4'-azodiphenylamine, 3,5-diaminobenzoic acid, 1-hexadecyloxy -2,4-phenylenediamine, 1-octadecyloxy-2,4-diaminobenzene, N,N'-bis(4-aminophenyl)piperazine, 4,4'-diaminodiphenyl sulfone, diaminobenzophenone, 3,5-diaminobenzoate, 2,2'-dimethyl-4,4'-diaminobiphenyl, 1,2-bis(4-aminophenoxy)ethane, 1,2-(4-aminophenoxy-4'-aminobiphenyloxy)ethane;
[0022] In the diamine compound, the molar ratio of diamine to diamine B is (3:7) to (2:3).
[0023] Further, the tetracarboxylic acid derivative is any one or more of cyclobutanetetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,3-dimethyl-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, pyromellitic dianhydride, 4,4'-biphenyl ether dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, bisphenol A type diether dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 3,3,4,4-diphenyl sulfone tetracarboxylic dianhydride, and 2,2'-difluoromethyl-4,4',5,5'-biphenyltetracarboxylic dianhydride.
[0024] Furthermore, the solvent is any one or more combinations of N-methylpyrrolidone, γ-butyrolactone, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, diethylene glycol butyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol dimethyl ether, ethylene glycol methyl ethyl ether, ethylene glycol dimethyl ether, diacetone alcohol, cyclohexanone, and cyclopentanone.
[0025] Furthermore, the molar ratio of the diamine compound to the tetracarboxylic acid derivative is (1:2) to (10:1).
[0026] Furthermore, the solid content of the polyamic acid solution is 5 to 10 wt %;
[0027] The viscosity of the polyamic acid solution is 25-35 mPa·s.
[0028] The embodiment of the third aspect of the present invention provides a polyimide, which is prepared by dehydration and ring closure of the polyamic acid described in the embodiment of the second aspect of the present invention.
[0029] The embodiment of the fourth aspect of the present invention provides a liquid crystal alignment agent, which includes any one or more of the polyamic acid described in the embodiment of the second aspect of the present invention or the polyimide described in the embodiment of the third aspect of the present invention mixed in any proportion.
[0030] The embodiment of the fifth aspect of the present invention provides a liquid crystal alignment film, and the liquid crystal alignment film is made of the liquid crystal alignment agent described in the embodiment of the fourth aspect of the present invention.
[0031] Compared with the prior art, the present invention has the following beneficial effects:
[0032] 1. In the present invention, the diamine contains a 2,5-diaminoaniline-1,3,4-oxadiazole structure. The diamine having the structure shown in Formula I can be used as a raw material for polyamic acid. The prepared polyamic acid is dehydrated to obtain polyimide. The prepared polyamic acid or polyimide can be used as a raw material for a liquid crystal alignment agent. Therefore, the liquid crystal alignment agent contains a 2,5-diaminoaniline-1,3,4-oxadiazole structure monomer. Since there are four nitrogen atoms between the two anilines of the diamine of this structure, they are combined with oxygen atoms to form a four-nitrogen-one-oxygen effect, which has a strong ability to absorb light carriers, absorbs ultraviolet light energy and transitions to an excited state of a higher energy level, with both π→π* and n→σ* transitions, and then the excited state electrons return to the ground state and release energy to cyclobutane, decomposing cyclobutane, thereby forming excellent alignment performance.
[0033] 2. In the present invention, the prepared liquid crystal alignment film still has good alignment function under low ultraviolet light exposure. BRIEF DESCRIPTION OF THE DRAWINGS
[0034] The drawings described herein are used to provide a further understanding of the present invention and constitute a part of this application. The exemplary embodiments of the present invention and their descriptions are used to explain the present invention and do not constitute an improper limitation of the present invention. In the drawings:
[0035] Figure 1 It is a graph showing the RDC afterimage test results of the liquid crystal display elements prepared in groups 1 to 9 in the experimental example of the present invention. DETAILED DESCRIPTION
[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0037] In a first aspect, the present invention provides a diamine having a structure shown in formula (I):
[0038]
[0039] Wherein, R1 and R2 are independently any one of hydrogen atom, halogen, -CF3, C1-C18 alkyl, -OCH3, -OC2H5, -COOCH3, aromatic compound containing 1-5 benzene rings or compound containing 1-5 heterocyclic rings;
[0040] X1 and X2 are each independently a single bond, -CH2-, -CH2CH2-, -C2H4-, -C(CH3)2-, -CH2O-, -CH2OCH2-, -HNCO-,
[0041] Any of the following:
[0042] m and n are any integers between 0 and 4 respectively.
[0043] It can be seen from the structure of formula (I) of the diamine that the diamine contains a 2,5-diaminoanilino-1,3,4-oxadiazole structure.
[0044] Specifically, the diamine is selected from any one or more combinations of the following compounds, the following compounds are structural formulas of compounds that can be listed, including but not limited to:
[0045]
[0046]
[0047]
[0048] In a second aspect, the present invention provides a polyamic acid, which is obtained by mixing a diamine compound, a tetracarboxylic acid derivative and a solvent, and then reacting to obtain a polyamic acid solution including polyamic acid; wherein the molar ratio of the diamine compound to the tetracarboxylic acid derivative is (1:2) to (10:1);
[0049] The solid content of the polyamic acid solution is 5 to 10 wt %;
[0050] The viscosity of the polyamic acid solution is 25 to 35 mPa·s.
[0051] The diamine compound includes the diamine provided by the embodiment of the first aspect of the present invention and diamine B;
[0052] Among them, diamine B is 1,2-diaminoethane, 1,3-diaminopropane, 1,4-diaminobutane, 1,6-diaminohexane, p-phenylenediamine, 1,5-naphthalenediamine, 1,8-diaminonaphthalene, 4,4'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylamine, 4,4'-azodiphenylamine, 3,5-diaminobenzoic acid, 1-hexadecyloxy -2,4-phenylenediamine, 1-octadecyloxy-2,4-diaminobenzene, N,N'-bis(4-aminophenyl)piperazine, 4,4'-diaminodiphenyl sulfone, diaminobenzophenone, 3,5-diaminobenzoate, 2,2'-dimethyl-4,4'-diaminobiphenyl, 1,2-bis(4-aminophenoxy)ethane, 1,2-(4-aminophenoxy-4'-aminobiphenyloxy)ethane;
[0053] In the diamine compound, the molar ratio of diamine to diamine B is (3:7) to (2:3);
[0054] Wherein, the tetracarboxylic acid derivative is any one or more of cyclobutanetetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,3-dimethyl-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, pyromellitic dianhydride, 4,4'-biphenyl ether dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, bisphenol A type diether dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 3,3,4,4-diphenylsulfonetetracarboxylic dianhydride, and 2,2'-difluoromethyl-4,4',5,5'-biphenyltetracarboxylic dianhydride.
[0055] The solvent is any one or more combinations of N-methylpyrrolidone, γ-butyrolactone, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, diethylene glycol butyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol dimethyl ether, ethylene glycol methyl ethyl ether, ethylene glycol dimethyl ether, diacetone alcohol, cyclohexanone, and cyclopentanone.
[0056] In a third aspect, the present invention provides a polyimide, which is prepared by dehydration and ring closure of the polyamic acid provided by the embodiment of the second aspect of the present invention.
[0057] In a fourth aspect, the present invention provides a liquid crystal alignment agent, which includes any one or more of the polyamic acid provided in the embodiment of the second aspect of the present invention or the polyimide provided in the embodiment of the third aspect of the present invention mixed in any proportion.
[0058] In a fifth aspect, the present invention provides a liquid crystal alignment film, which is made from the liquid crystal alignment agent provided by the embodiment of the fourth aspect of the present invention.
[0059] The present invention will now be further explained with reference to the embodiments.
[0060] Unless otherwise specified, the raw materials in the preparation examples, synthesis examples, embodiments and comparative examples in this application can be obtained from commercial sources.
[0061] Preparation Examples 1 to 3 are the preparation of diamines, which are specifically as follows:
[0062] Preparation Example 1
[0063] S1: Add p-nitrochlorobenzene (49.455 g), sodium hydroxide (4 g, 0.1 mol), and 1,4-dioxane (161 g) into a 500 mL three-necked flask, and heat to 80° C. while stirring to prepare a mixture; dropwise add 2,5-diamino-1,3,4-oxadiazole (15.164 g) dissolved in 1,4-dioxane (100 g) into the above mixture, and drip the 2,5-diamino-1,3,4-oxadiazole over 4 hours; during the dripping process, add sodium hydroxide (4 g) every 1 hour. , add sodium hydroxide (16g) in total; after adding 2,5-diamino-1,3,4-oxadiazole, heat to 100℃, stir and react for 4 hours, after the reaction is completed, cool to room temperature (25℃), add water (1300g) to precipitate crystals, filter to obtain the product, and then dry to obtain a crude product (49.15g); add the above crude product to THF (150g), stir, heat to reflux for 30min, cool in an ice water bath while stirring, add high-purity water (150g) to recrystallize the product. Filter it again, and dry the product obtained after filtration to obtain TA-1-1 (46.91g), with a purity of 94.4% and a yield of 86.23%.
[0064] S2: Add the above-obtained TA-1-1 (45 g) and DMF (180 g) to a 500 mL three-necked flask, then add palladium carbon catalyst (3 g, 5% palladium carbon catalyst wet basis, water content 50%), stir and heat at 100 ° C, add hydrated hydrazine (40 g) dropwise for 4 hours, and continue to heat and stir at 100 ° C for 2 hours after the hydrated hydrazine is added. After the reaction is completed, filter and remove the palladium carbon catalyst while hot, add high-purity water (180 g) to the filtrate and stir, cool to 25 ° C to precipitate solid, filter it, and dry the obtained product to obtain a crude product (32.6 g); add the above-mentioned crude product to DMF (90 g), heat and stir at 80 ° C for 30 min, then cool in an ice-water bath, add ethanol (90 g) for recrystallization, filter it, and finally dry the crystals to obtain TA-1 (31.59 g) with a purity of 99% and a yield of 89.32%.
[0065] In this preparation example, the synthetic route can be expressed as follows:
[0066]
[0067] High-resolution mass spectrometry of the prepared compound TA-1, ESI source, positive ion mode, molecular formula is C 14 H 14 N6O, theoretical value 282.12, test value 282.13. Elemental analysis (C 14 H 14 N6O), theoretical value C: 59.56, H: 5.00, N: 29.11, O: 5.67, measured value C: 59.57, H: 5.00, N: 29.12, O: 5.65.
[0068] Preparation Example 2
[0069] S1: Add 4'-chloro-4-nitro-diphenyl ether (52.96 g), sodium hydroxide (2 g), and DMSO (150 g) into a 500 ml three-necked flask, and heat to 85° C. while stirring to prepare a mixture; dropwise add 2,5-diamino-1,3,4-oxadiazole (10.11 g) dissolved in DMSO (100 g) into the above mixture, and drip the 2,5-diamino-1,3,4-oxadiazole over 5 hours; add sodium hydroxide (2 g) every hour; add a total of sodium hydroxide (10 g); add 2,5-diamino-1,3,4-oxadiazole over 5 hours; After the oxadiazole, heat to 120°C and stir to react for 2 hours; after the reaction is completed, cool to room temperature (25°C), add water (1000g) to precipitate crystals, filter to obtain the product, and dry to obtain a crude product (48.12g); add the above crude product to DMF (145g), stir, heat to 80°C, cool in an ice water bath while stirring, add high-purity water (145g) to recrystallize the product; filter it, and dry the obtained product to obtain TA-2-1 (45.49g), with a purity of 96.3% and a yield of 83.23%;
[0070] S2: Add the above-obtained TA-2-1 (43 g) and DMF (160 g) to a 500 mL three-necked flask, then add palladium carbon catalyst (3 g, 5% palladium carbon catalyst wet basis, water content 50%), stir and heat at 100°C, add hydrated hydrazine (32 g) dropwise for 4 hours, and continue to heat and stir at 100°C for 2 hours after the hydrated hydrazine is added; after the reaction is completed, filter and remove the catalyst while hot, add high-purity water (160 g) to the filtrate and stir, cool to 25°C to precipitate solid, filter it, and dry the obtained product to obtain a crude product (34.35 g); add the above-mentioned crude product to DMF (100 g), heat and stir at 80°C for 30 min, then cool in an ice-water bath, add methanol (100 g) for recrystallization; filter it, dry the crystals to obtain TA-2 (32.46 g) with a purity of 99% and a yield of 87.56%.
[0071] In this preparation example, the synthetic route can be expressed as follows:
[0072]
[0073] High-resolution mass spectrum of the prepared compound TA-2, ESI source, positive ion mode, molecular formula C 26 H 22 N6O3, theoretical value 466.18, test value 466.17. Elemental analysis (C 26 H 22 N6O3), theoretical value C: 66.94, H: 4.75, N: 18.02, O: 10.29, measured value C: 66.93, H: 5.00, N: 18.01, O: 10.31.
[0074] Preparation Example 3
[0075] S1: Add p-nitrobenzoyl chloride (38.97 g), TA-1 (28.23 g), and DMF (260 g) to a 500 mL three-necked flask, stir, and place in an ice-water bath to 4°C to prepare a mixture; slowly add triethylamine to the above mixture, drip the triethylamine in 1 hour, heat to 80°C, and stir to react for 5 hours; after the reaction is completed, cool to room temperature (25°C), add water (1200 g) to precipitate crystals, filter to obtain the product, and then dry to obtain a crude product (55.46 g); add the above crude product to DMF (150 g), heat to 80°C and stir, stir to react for 30 minutes, after the reaction is completed, cool in an ice-water bath while stirring, add high-purity water (150 g) to recrystallize the product; filter it, and dry the obtained product to obtain TA-3-1 (53.86 g), with a purity of 95.6% and a yield of 88.7%;
[0076] S2: Add the above-obtained TA-3-1 (50 g) and DMF (200 g) to a 500 mL three-necked flask, then add palladium carbon catalyst (4 g, 5% palladium carbon catalyst wet basis, water content 50%), stir and heat at 100°C, add hydrated hydrazine (32 g) dropwise for 4 hours, and continue to heat and stir at 100°C for 2 hours after the hydrated hydrazine is added; after the reaction is completed, filter and remove the catalyst while hot, add high-purity water (200 g) to the filtrate and stir, cool to 25°C to precipitate solids, filter it, and dry the obtained product to obtain a crude product (39.62 g); add the above-mentioned crude product to DMF (90 g), heat and stir at 80°C for 30 min, then cool in an ice-water bath, add ethanol (90 g) for recrystallization; filter it, dry the crystals to obtain TA-3 (35.41 g) with a purity of 99% and a yield of 81.8%.
[0077] In this preparation example, the synthetic route can be expressed as follows:
[0078]
[0079] High-resolution mass spectrum of the compound TA-3, ESI source, positive ion mode, molecular formula C 28 H 24 N8O3, theoretical value 520.2, test value 520.21. Elemental analysis (C 28 H 24 N8O3), theoretical value C: 64.61, H: 4.65, N: 21.53, O: 9.22, measured value C: 64.60, H: 4.65, N: 21.53, O: 9.21.
[0080] The following are the abbreviations and structures of the compounds used in the synthesis examples, embodiments and comparative examples, as follows:
[0081] A-1: p-phenylenediamine, the structural formula is as follows:
[0082]
[0083] A-2: 1,2-bis(4-aminophenoxy)ethane, the structural formula is as follows:
[0084]
[0085] A-3: 1,2-(4-aminophenoxy-4'-aminobiphenyloxy)ethane, the structural formula is as follows:
[0086]
[0087] A-4: 4,4'-diaminodiphenylmethane, the structural formula is as follows:
[0088]
[0089] A-5: 4,4'-diaminodiphenylamine, the structural formula is as follows:
[0090]
[0091] A-6: 4,4'-diaminodiphenyl ether, the structural formula is as follows:
[0092]
[0093] TA-1, the structural formula is as follows:
[0094]
[0095] TA-2, the structural formula is as follows:
[0096]
[0097] TA-3, the structural formula is as follows:
[0098]
[0099] B-1: Cyclobutanetetracarboxylic dianhydride (CBDA), the structural formula is as follows:
[0100]
[0101] B-2: 3,3',4,4'-biphenyltetracarboxylic dianhydride (BPDA), the structural formula is as follows:
[0102]
[0103] In the following synthesis examples, NMP is N-methylpyrrolidone; BCS is ethylene glycol monobutyl ether.
[0104] Synthesis example 1
[0105] In a 250 mL reaction container equipped with a stirring device and a nitrogen inlet tube, NMP (71.12 g), TA-1 (2.541 g, 9 mmol), A-1 (0.973 g, 9 mmol), A-2 (1.466 g, 6 mmol), and A-3 (1.922 g, 6 mmol) were added respectively, and stirred while passing nitrogen to completely dissolve. Then, B-1 (5.648 g, 28.8 mmol) was added, and stirred at 25° C. for 4 hours. NMP (117.13 g) and BCS (50.2 g) were added to prepare a polyamic acid solution (PAA-1) with a solid content of 5 wt%, a BCS content of 20 wt%, and the rest being NMP; the viscosity of the polyamic acid solution was 26 mPa·s.
[0106] Synthesis example 2
[0107] In a 250 mL reaction container equipped with a stirring device and a nitrogen inlet tube, NMP (66.67 g), TA-1 (2.823 g, 10 mmol), A-2 (1.832 g, 7.5 mmol), and A-3 (2.403 g, 7.5 mmol) were added respectively, and stirred while passing nitrogen to completely dissolve them. Then, B-1 (4.707 g, 24 mmol) was added, and stirred at 25°C for 4 hours. NMP (109.8 g) and BCS (47.1 g) were added to prepare a polyamic acid solution (PAA-2) with a solid content of 5 wt%, a BCS content of 20 wt%, and the rest being NMP. The viscosity of the polyamic acid solution was 31 mPa·s.
[0108] Synthesis example 3
[0109] In a 250 mL reaction container equipped with a stirring device and a nitrogen inlet tube, NMP (64.29 g), TA-1 (2.823 g, 10 mmol), A-2 (1.221 g, 5 mmol), A-3 (1.602 g, 5 mmol), and A-4 (0.991 g, 5 mmol) were added respectively, and stirred while passing nitrogen to completely dissolve them. Then, B-1 (4.707 g, 24 mmol) was added, and stirred at 25°C for 4 hours. NMP (106.88 g) and BCS (45.37 g) were added to prepare a polyamic acid solution (PAA-3) with a solid content of 5 wt%, a BCS content of 20 wt%, and the rest being NMP. The viscosity of the polyamic acid solution was 29 mPa·s.
[0110] Synthesis example 4
[0111] In a 250 mL reaction container equipped with a stirring device and a nitrogen inlet tube, NMP (61.68 g), TA-2 (3.732 g, 8 mmol), A-2 (1.466 g, 6 mmol), and A-3 (1.922 g, 6 mmol) were added respectively, and stirred while passing nitrogen to completely dissolve them. Then, B-1 (3.765 g, 19.2 mmol) was added, and stirred at 25°C for 4 hours. 101.6 g NMP and BCS (43.54 g) were added to prepare a polyamic acid solution (PAA-4) with a solid content of 5 wt%, a BCS content of 20 wt%, and the rest being NMP. The viscosity of the polyamic acid solution was 28 mPa·s.
[0112] Synthesis example 5
[0113] In a 250 mL reaction container equipped with a stirring device and a nitrogen inlet tube, NMP (64.13 g), TA-3 (4.164 g, 8 mmol), A-2 (1.466 g, 6 mmol), and A-3 (1.922 g, 6 mmol) were added respectively, and stirred while passing nitrogen to completely dissolve them. Then, B-1 (3.765 g, 19.2 mmol) was added, and stirred at 25°C for 4 hours. NMP (105.63 g) and BCS (45.27 g) were added to prepare a polyamic acid solution (PAA-5) with a solid content of 5 wt%, a BCS content of 20 wt%, and the rest being NMP. The viscosity of the polyamic acid solution was 27 mPa·s.
[0114] Synthesis example 6
[0115] In a 250 mL reaction container equipped with a stirring device and a nitrogen inlet tube, NMP (56.8 g), A-1 (1.081 g, 10 mmol), A-2 (1.832 g, 7.5 mmol), and A-3 (2.403 g, 7.5 mmol) were added respectively, and stirred while passing nitrogen to completely dissolve them. Then, B-1 (4.707 g, 24 mmol) was added, and stirred at 25°C for 4 hours. NMP (93.55 g) and BCS (40.09 g) were added to prepare a polyamic acid solution (PAA-6) with a solid content of 5 wt%, a BCS content of 20 wt%, and the rest being NMP. The viscosity of the polyamic acid solution was 29 mPa·s.
[0116] Synthesis Example 7
[0117] In a 250 mL reaction container equipped with a stirring device and a nitrogen inlet tube, NMP (63.72 g), A-2 (1.832 g, 7.5 mmol), A-3 (3.204 g, 10 mmol), and A-6 (1.502 g, 7.5 mmol) were added respectively, and stirred while passing nitrogen to completely dissolve them. Then, B-1 (4.707 g, 24 mmol) was added, and stirred at 25°C for 4 hours. NMP (104.95 g) and BCS (44.98 g) were added to prepare a polyamic acid solution with a solid content of 5 wt%, a BCS content of 20 wt%, and the rest being NMP. The viscosity of the polyamic acid solution was 28 mPa·s.
[0118] Synthesis example 8
[0119] In a 250 mL reaction container equipped with a stirring device and a nitrogen inlet tube, NMP (68.21 g), A-4 (0.991 g, 5 mmol), and A-5 (3.985 g, 20 mmol) were added respectively, and stirred while passing nitrogen to completely dissolve them. Then, B-2 (7.061 g, 24 mmol) was added, and stirred at 25°C for 4 hours. NMP (112.35 g) and BCS (48.15 g) were added to prepare a polyamic acid solution with a solid content of 5 wt%, a BCS content of 20 wt%, and the rest being NMP. The viscosity of the polyamic acid solution was 33 mPa·s.
[0120] In Synthesis Examples 1 to 8, in the process of synthesizing polyamic acid, the types and molar fractions of various raw materials are shown in Table 1;
[0121] Since the diamine compound includes diamine and diamine B, the number in the bracket represents the molar fraction of the substance in the diamine compound.
[0122] Table 1
[0123]
[0124] Examples 1 to 5 and Comparative Examples 1 to 3 provide preparation methods of liquid crystal alignment agents, which are specifically as follows.
[0125] Example 1
[0126] The present embodiment provides a method for preparing an alignment agent, which comprises the following steps: adding a polymer component into a 50 mL three-necked flask, wherein the polymer component comprises a polyamic acid solution A and a polyamic acid solution B, wherein the polyamic acid solution A is the polyamic acid solution (PAA-1) (8 g) obtained in Synthesis Example 1, and the polyamic acid solution B is the polyamic acid solution (PAA-8) (12 g) obtained in Synthesis Example 8, and stirring at 25° C. for 30 min, thereby obtaining a liquid crystal alignment agent (AL-1).
[0127] In Examples 2 to 5 and Comparative Examples 1 to 3, the preparation method of the alignment agent provided is the same as that of Example 1, and the difference from Example 1 is that different polyamic acid solutions are used in Examples 2 to 5 and Comparative Examples 1 to 3. The types of polyamic acid solutions used in Examples 2 to 5 and Comparative Examples 1 to 3 are shown in Table 2;
[0128] The data in brackets indicate the mass percentage content of the substance in the polymer component.
[0129] Table 2
[0130]
[0131] Experimental Example 1
[0132] This experimental example provides the preparation of a liquid crystal alignment film and a liquid crystal cell. The specific steps are as follows:
[0133] S1: Preparation of liquid crystal alignment film
[0134] Two glass substrates of 3 cm×4 cm and 0.5 mm in thickness were prepared, wherein the lower glass substrate had a comb-shaped ITO electrode with a width of 10 μm, a spacing of 10 μm between adjacent comb-shaped electrodes, and the pixel electrodes and the common electrodes were arranged in a cross pattern; the upper glass substrate had no electrode, and the liquid crystal alignment agent prepared in the embodiment and the comparative example was coated on the two glass substrates, and subjected to pre-baking at 100° C. for 3 min and main curing (oven, 230° C. for 20 min), to obtain a liquid crystal alignment film with a thickness of 100 nm;
[0135] S2: Preparation of liquid crystal cell
[0136] In Experimental Example 1, the upper and lower glass substrates with liquid crystal alignment films were irradiated with polarized ultraviolet rays through a 254nm band filter and a polarizer, and further baked in an oven at 230°C to remove small molecules generated during the photo-alignment process. A 4μm spacer was sprayed on the side of the upper glass substrate with the liquid crystal alignment film, and a certain pattern of frame-sealing glue was scratched on the lower glass substrate. The upper and lower glass substrates were pre-laminated with the sides of the liquid crystal alignment films facing each other and the rubbing directions were parallel, and then placed in a vacuum laminating machine for vacuuming and laminating. After laminating, the frame-sealing glue was cured by baking on a 150°C hot plate for 60 minutes, and the liquid crystal was poured in by decompression, and then sealed with a light-curing glue to obtain a liquid crystal box.
[0137] Experimental Example 2
[0138] The performance of the liquid crystal alignment film and the liquid crystal box prepared according to the operating steps in Experimental Example 1 were tested for the liquid crystal alignment agents provided in the embodiments and comparative examples. The relevant testing parameters and testing methods are as follows.
[0139] 1. Characterization of friction resistance of liquid crystal alignment film
[0140] The friction resistance of the liquid crystal alignment film can be tested by rubbing the liquid crystal alignment film with a friction machine and testing the haze of the liquid crystal alignment film after rubbing. To be more specific, the testing method of the friction resistance is as follows:
[0141] The liquid crystal alignment agent is coated on an ITO glass substrate of 80×80 mm, and after pre-baking at 100°C for 3 min and main curing (oven, 230°C for 30 min), a polyimide alignment film with a thickness of 100 nm, i.e., a liquid crystal alignment film, is obtained; the liquid crystal alignment film is rubbed 50 times on a friction machine with a pressing amount of 0.5 mm, and the haze value of the liquid crystal alignment film is obtained by detecting with a haze meter after the friction is completed.
[0142] Among them, the quality of friction resistance is characterized by the following parameters:
[0143] ◎: Haze value ≤ 0.2, excellent friction resistance;
[0144] ○: 0.2<haze value≤0.5, good friction resistance;
[0145] △: 0.5<haze value, poor friction resistance
[0146] 2. Characterization of contrast
[0147] The contrast ratio was tested after the liquid crystal display element (liquid crystal box with polarizing plate attached) manufactured in Experimental Example 1 was driven with saturated AC voltage for 24 hours. The test instrument was a brightness meter (device model: CA310), and the liquid crystal display element was tested under a polarizing microscope. The minimum brightness of the test was taken as the blackness. An arbitrary rectangular wave voltage was applied to the liquid crystal display element, and the maximum brightness was tested as the whiteness. The contrast ratio is defined as the ratio of whiteness to blackness.
[0148] The contrast evaluation results of the liquid crystal display element are as follows:
[0149] ◎: Contrast ≥ 1200, the contrast of the liquid crystal display element is good;
[0150] ○: 800 ≤ contrast < 1200, the contrast of the liquid crystal display element is average;
[0151] △: Contrast ratio <800, the contrast ratio of the liquid crystal display element is poor.
[0152] 3. Evaluation of residual image performance of liquid crystal alignment film
[0153] The residual image performance of the liquid crystal alignment film can be evaluated by the residual voltage of the liquid crystal display element (hereinafter referred to as RDC). Specifically, the residual voltage of the liquid crystal display element is detected as follows: a DC voltage of 5V is applied to the liquid crystal display element prepared in Experimental Example 1 at a temperature of 60°C for 1 hour, and then the applied voltage is removed, the pixel electrode and the common electrode are short-circuited for 1 second, and then the residual voltage between the two electrodes is immediately tested for 600 seconds;
[0154] The evaluation criteria for RDC are as follows:
[0155] ◎: RDC≤0.2V, excellent afterimage performance;
[0156] ○: 0.2V<RDC≤0.6V, good afterimage performance;
[0157] △: RDC>0.6V, poor afterimage performance.
[0158] 4. Performance evaluation of VHR voltage holding rate
[0159] The conditions for testing VHR are: at a temperature of 60°C, a 5V voltage is applied to the liquid crystal box, and after 60us, the initial voltage V1=5V; the voltage is disconnected, and the residual voltage V2 of the liquid crystal box is measured 167ms after the voltage is disconnected, VHR=V2 / V1*100%.
[0160] The evaluation criteria for VHR are as follows:
[0161] ◎: VHR≥98%, excellent voltage holding rate performance;
[0162] ○: 98%>VHR≥95%, voltage holding rate performance is average;
[0163] △: 95%>VHR, the voltage holding rate is poor.
[0164] 5. Orientation performance of liquid crystal alignment film
[0165] The alignment performance of the liquid crystal alignment film can be determined by measuring the pretilt angle of the liquid crystal using an OPTIPRO instrument on the manufactured liquid crystal display element.
[0166] The evaluation criteria for orientation performance are as follows:
[0167] ◎: 2°>pretilt angle>0.05°, normal orientation;
[0168] △: If the pretilt angle is less than 0.05° or greater than 2°, poor orientation will occur.
[0169] The test results of the above performance parameters are shown in Table 3;
[0170] Among them, Group 7 and Group 8 both use the liquid crystal alignment agent prepared in Comparative Example 2 as the raw material for preparing the liquid crystal alignment film and the liquid crystal box in Experimental Example 1. The difference between the two is that the ultraviolet irradiation amount used in Group 7 is 200mJ / cm 2 The UV irradiation dose used in Group 8 was 500 mJ / cm 2 .
[0171] Table 3
[0172]
[0173]
[0174] It can be seen from the data in Table 3 that the liquid crystal alignment agents provided in Examples 1 to 5 contain diamines with a 2,5-diaminoaniline-1,3,4-oxadiazole structure, and the liquid crystal display elements prepared using the liquid crystal alignment agents as raw materials have excellent orientation performance, significant voltage holding rate performance, good friction resistance, excellent contrast and good afterimage performance. Their comprehensive performance is better than that of the liquid crystal display elements prepared using the liquid crystal alignment agents provided in Comparative Examples 1 to 3 as raw materials. Among them, the liquid crystal display elements of Group 6 and Group 7, which are prepared using the liquid crystal alignment agents provided in Comparative Examples 1 and 2 as raw materials, respectively, have poor orientation, which makes it impossible to measure the contrast performance.
[0175] In addition, it can be seen from the data in Table 3 that at low UV exposure (200mJ / cm 2 ), in the first group of data, the liquid crystal alignment agent provided in Example 1 has excellent orientation performance due to the diamine containing a 2,5-diaminoaniline-1,3,4-oxadiazole structure; while in the sixth group of data, the liquid crystal alignment agent provided by Comparative Example 1 does not use a diamine containing a 2,5-diaminoaniline-1,3,4-oxadiazole structure, and the type of diamine B used is consistent with the type of diamine B in Example 1. The liquid crystal display element prepared using the liquid crystal alignment agent as a raw material has poor orientation. This shows that the liquid crystal display element prepared using the liquid crystal alignment agents provided in Examples 1 to 5 as raw materials still has excellent orientation performance under low ultraviolet irradiation.
[0176] In addition, the RDC afterimage test results of the liquid crystal display elements prepared in groups 1 to 9 are as follows: Figure 1 As shown, Figure 1 The results show that the liquid crystal display element prepared by using the liquid crystal alignment agent provided in Examples 1-5 as a raw material can release residual charges without causing residual images.
[0177] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0178] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A diamine, characterized in that The diamine has a structure shown in formula (I): Wherein, R1 and R2 are independently any one of hydrogen atom, halogen, -CF3, C1-C18 alkyl, -OCH3, -OC2H5, -COOCH3, aromatic compound containing 1-5 benzene rings or compound containing 1-5 heterocyclic rings; X1 and X2 are each independently a single bond, -CH2-, -CH2CH2-, -C2H4-, -C(CH3)2-, -CH2O-, -CH2OCH2-, -HNCO-, Any of the following; m and n are any integers between 0 and 4 respectively.
2. A diamine according to claim 1, characterized in that, The diamine is selected from any one or more combinations of compounds represented by the following formulas (1-1) to (1-22); 3. A polyamic acid, characterized in that A polyamic acid solution including the polyamic acid is obtained by mixing a diamine compound, a tetracarboxylic acid derivative and a solvent and reacting the mixture; The diamine compound includes the diamine according to any one of claims 1 or 2.
4. A polyamic acid according to claim 3, characterized in that: The diamine compound also includes diamine B; The diamine B is 1,2-diaminoethane, 1,3-diaminopropane, 1,4-diaminobutane, 1,6-diaminohexane, p-phenylenediamine, 1,5-naphthalenediamine, 1,8-diaminonaphthalene, 4,4'-diaminodiphenylmethane, 1,4-bis(4-aminophenoxy)benzene, 4,4'-diaminodiphenyl ether, 4,4'-diaminodiphenylamine, 4,4'-azodiphenylamine, 3,5-diaminobenzoic acid, 1-hexadecyloxy -2,4-phenylenediamine, 1-octadecyloxy-2,4-diaminobenzene, N,N'-bis(4-aminophenyl)piperazine, 4,4'-diaminodiphenyl sulfone, diaminobenzophenone, 3,5-diaminobenzoate, 2,2'-dimethyl-4,4'-diaminobiphenyl, 1,2-bis(4-aminophenoxy)ethane, 1,2-(4-aminophenoxy-4'-aminobiphenyloxy)ethane; In the diamine compound, the molar ratio of diamine to diamine B is (3:7) to (2:3).
5. A polyamic acid according to claim 3, characterized in that: The tetracarboxylic acid derivative is any one or more of cyclobutanetetracarboxylic dianhydride, 1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,3-dimethyl-cyclobutanetetracarboxylic dianhydride, 1,2,3,4-tetramethyl-1,2,3,4-cyclobutanetetracarboxylic dianhydride, 1,4,5,8-naphthalenetetracarboxylic dianhydride, pyromellitic dianhydride, 4,4'-biphenyl ether dianhydride, 3,3',4,4'-biphenyltetracarboxylic dianhydride, bisphenol A type diether dianhydride, 9,9-bis(3,4-dicarboxyphenyl)fluorene dianhydride, 3,3,4,4-diphenylsulfonetetracarboxylic dianhydride, and 2,2'-difluoromethyl-4,4',5,5'-biphenyltetracarboxylic dianhydride. The solvent is any one or more combinations of N-methylpyrrolidone, γ-butyrolactone, dimethyl sulfoxide, N,N-dimethylformamide, N,N-dimethylacetamide, diethylene glycol butyl ether, ethylene glycol monoethyl ether, ethylene glycol monobutyl ether, diethylene glycol dimethyl ether, ethylene glycol methyl ethyl ether, ethylene glycol dimethyl ether, diacetone alcohol, cyclohexanone, and cyclopentanone.
6. A polyamic acid according to claim 3, characterized in that: The molar ratio of the diamine compound to the tetracarboxylic acid derivative is (1:2) to (10:1).
7. A polyamic acid according to claim 3, characterized in that: The solid content of the polyamic acid solution is 5 to 10 wt %; The viscosity of the polyamic acid solution is 25-35 mPa·s.
8. A polyimide, characterized in that: The polyimide is prepared by dehydration and ring closure of the polyamic acid described in any one of claims 3 to 7.
9. A liquid crystal alignment agent, characterized in that: The invention comprises any one or more of the polyamic acid according to any one of claims 3 to 7 or the polyimide according to claim 8 mixed in any proportion.
10. A liquid crystal alignment film, characterized in that: The liquid crystal alignment film is made from the liquid crystal alignment agent according to claim 9.