Asymmetric medium-band-gap fused ring acceptor material and photovoltaic application thereof
By introducing alkoxy side chains and weak electron-absorbing end groups into the fused ring acceptor material, asymmetric medium bandgap fused ring acceptor materials are developed, which solves the problem of insufficient medium bandgap acceptor materials in the prior art, and realizes the High-efficiency organic solar cells and indoor photovoltaic devices have improved performance.
Patent Information
- Application Number
- CN202310668340.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-06
AI Technical Summary
The lack of efficient medium bandgap acceptor materials in existing organic solar cells limits the improvement of device efficiency, especially the lag in performance development of the former battery, which affects the performance of the entire solar cell system.
A class of asymmetric medium band gap fused ring acceptor materials were developed, and the synthetic routes such as Stille coupling reaction, Vilsmeier-Haack reaction and Knoevenagel condensation reaction were used to introduce alkoxy side chains and weak electron-absorbing end groups into the fused ring structure. , an acceptor material with high light absorption coefficient and excellent photovoltaic properties were prepared.
High-efficiency stacked organic solar cells and indoor photovoltaic devices are achieved, which improves open circuit voltage, short circuit current density and fill factor, with an efficiency of more than 20%, and shows excellent energy conversion efficiency under indoor light.
Smart Images

Figure CN119080802A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of organic solar cell material preparation, relates to a class of organic solar cell receptor materials, specifically to a class of medium-bandgap condensed ring receptor materials containing an asymmetric condensed ring structure, and also to applications in laminated organic solar cells and indoor photovoltaic devices. Background Art
[0002] As energy problems become increasingly serious, the development of new energy sources is urgent. Solar energy has great development prospects due to its many advantages such as clean, pollution-free, inexhaustible and inexhaustible. How to better utilize solar energy is an effective solution to the energy crisis. In the past three decades, organic solar cells (OSCs) have attracted much attention due to their low manufacturing cost, good mechanical flexibility and light weight. The rapid development of organic solar cells is mainly due to the continuous innovation of donor and acceptor materials in recent years. At present, the power conversion efficiency of single-junction devices and tandem devices exceeds 19% and 20%, respectively (Adv. Mater., 2021, 33, e2102420; Joule., 2022, 6, 171-184). However, compared with commercial silicon-based solar cells and high-efficiency perovskite solar cells, the device efficiency of OSCs still needs to be further improved.
[0003] In order to further improve the efficiency of OSCs, it is urgent to develop tandem solar cells (tandem solar cells consist of a front cell with wide bandgap absorption and a rear cell with narrow bandgap absorption). Acceptor materials with narrow bandgap absorption characteristics have been widely studied, and the device efficiency has exceeded 19%. However, the research on medium-bandgap acceptor materials for the preparation of high-efficiency front cells is still lagging behind, and it is urgent to develop excellent medium-bandgap acceptor materials to improve the performance of the front cell.
[0004] At present, the research on medium-bandgap acceptor materials has not received enough attention. Through literature research, it was found that there are only a few reports on such materials (Adv. Mater. 2017, 29, 1700254; Chem. Mater. 2019, 31, 3941-3947; Joule. 2021, 5, 1231-1245; Adv. Mater. 2022, 34, e2108090). Therefore, it is very necessary to develop more efficient medium-bandgap acceptor materials. In the study, we found that based on the classic A-DA′DA type condensed ring structure, the condensed ring structure was modified with an alkyl side chain containing an oxygen atom, and then combined with a weak electron-withdrawing end group to effectively regulate the absorption of the material to obtain a medium-bandgap acceptor material. However, molecules with symmetrical structures generally have strong crystallinity, and the device morphology is difficult to be effectively controlled. Asymmetric strategy is an effective means to regulate molecular properties. In acceptor molecules, changes in structural symmetry not only affect the spectrum and energy level, but also enhance the molecular dipole and charge transfer capabilities. Moreover, the structural changes can adjust the molecular stacking and crystallinity of the material, and ultimately improve the compatibility of the donor and the acceptor. Therefore, in order to promote the efficiency improvement and commercial application of organic solar cells, we invented a class of asymmetric medium-bandgap fused ring acceptors, which realized high-efficiency tandem organic solar cells and indoor photovoltaic devices. Summary of the invention
[0005] The purpose of the present invention is to prepare a type of asymmetric medium band gap (E g ≈1.55–2.00eV) fused ring acceptor materials can be used as acceptors in the active layer of OSCs. Such materials have the advantages of high lowest unoccupied molecular orbital energy level (LUMO), light absorption range from near ultraviolet to visible light, and high device open circuit voltage. When used as acceptor materials in tandem organic solar cells and indoor photovoltaic devices, they can show excellent device performance, high open circuit voltage, short circuit current and fill factor. Therefore, such materials have good application prospects in the field of tandem organic solar cells and indoor photovoltaic devices.
[0006] The technical solution adopted by the present invention is: to provide a medium band gap acceptor material having both an asymmetric condensed ring structure containing an alkoxy side chain and a weak electron-withdrawing end group structure, wherein the structural feature of the condensed ring central core is: a thiophene unit containing an alkoxy side chain and a thiophene unit containing an alkoxy side chain are used as π bridges respectively, and a condensed ring center is formed with a conjugated structure containing a benzene ring, and both sides of the central core are connected to weak electron-withdrawing end groups, and the general structural formula thereof is shown in Formula I:
[0007]
[0008] in:
[0009] R1, R2, and R3 in the structural formula are independently selected from linear, branched, or alkyl-substituted aromatic side chains having 1 to 40 carbon atoms;
[0010] The Weak A unit is selected from any one of the following structural formulas:
[0011]
[0012] in:
[0013] The dotted line in the Weak A structure indicates the connection site to the Weak A unit.
[0014] Preferably, the Ar1 unit is selected from any one of the following structural formulas:
[0015]
[0016] Wherein, R4 in the Ar1 structural formula is independently selected from H, a linear or branched alkyl group having 1 to 20 carbon atoms, and the dotted line in the Ar1 structural formula represents the connection site with other units.
[0017] The preparation method of the compound comprises the following steps:
[0018] Its synthetic route is as follows:
[0019]
[0020] In the structural formula, R1, R2 and R3 are all straight chain, branched chain or alkyl-substituted aromatic side chains having 1 to 40 carbon atoms.
[0021] (1) Compound A, Compound B and Compound C are added to 80-100 mL of toluene, and then a catalyst, tetrakis(triphenylphosphine)palladium, is added. The mixture is reacted at 80-90° C. for 10-12 hours to obtain Compound D through a Stille coupling reaction;
[0022] (2) Under nitrogen protection, compound D and triphenylphosphine are added to o-dichlorobenzene, and then the system is heated to 160-180° C. for 16-18 hours to obtain compound E;
[0023] (3) Under nitrogen protection, compound E, halogenated alkane R3Br, potassium carbonate and potassium iodide are added to N,N-dimethylformamide, and reacted at 80-85°C for 10-12h to obtain compound F;
[0024] (4) This reaction is a Vilsmeier-Haack reaction. Compound F is dissolved in 1,2-dichloroethane and then added dropwise to the formylation agent phosphorus oxychloride under low temperature conditions. The molar ratio of compound 6 to phosphorus oxychloride is 1:10 to 1:30. After reacting at low temperature for 1 to 2 hours, the system is heated to 80 to 100°C and reacted for 8 to 12 hours to obtain compound G.
[0025] (5) This reaction is a Knoevenagel condensation reaction. Under nitrogen protection, compound G, Weak A and pyridine are reacted at 60°C for 5 to 8 hours to obtain compound H.
[0026] Compared with the prior art, the present invention has the following advantages:
[0027] (1) The present invention is the first to simultaneously utilize thiophene structures modified with alkoxy side chains and thiophene structures modified with alkoxy side chains as π-bridge units of fused ring acceptors in coordination with weak electron-withdrawing end groups to obtain an asymmetric medium band gap (E) with a high absorption coefficient. g ≈1.55–2.00 eV) fused ring acceptor materials. Their absorption range is in the near-ultraviolet and visible light regions, which is significantly blue-shifted compared to common narrow-bandgap acceptor materials.
[0028] (2) Compared with the symmetrical alkoxy side chain-strong electron-withdrawing end group structure, this type of material has a higher LUMO energy level, which can significantly increase the open circuit voltage of photovoltaic devices. In addition, the change in symmetry effectively regulates the crystallinity of the material, enhances the dipole and charge transfer capabilities, and enables the device to have a higher short-circuit current density and fill factor.
[0029] (3) The light absorption range of this type of material is complementary to that of the narrow-bandgap acceptor material and can provide a higher open-circuit voltage. When used as a front cell, it can achieve good light absorption complementarity and voltage superposition with the rear cell made of a narrow-bandgap acceptor material, thereby realizing a high-efficiency stacked organic solar cell (efficiency exceeding 20%).
[0030] (4) The light absorption range of this type of material has a good match with the emission spectrum of indoor lighting sources. Photovoltaic devices based on this type of receptor material exhibit excellent open-circuit voltage and energy conversion efficiency (efficiency exceeding 32%) under indoor light irradiation, and have important applications in indoor photovoltaic devices. BRIEF DESCRIPTION OF THE DRAWINGS
[0031] Figure 1 This is the thin film absorption spectrum of the receptor molecule ABTP-S.
[0032] Figure 2 This is the thin film absorption spectrum of the acceptor molecule ABTP-SCl.
[0033] Figure 3This is the thin film absorption spectrum of the acceptor molecule ABTP-4Cl.
[0034] Figure 4 This is the thin film absorption spectrum of the receptor molecule ABTP-4F.
[0035] Figure 5 This is the thin film absorption spectrum of the receptor molecule ABNP-S.
[0036] Figure 6 This is the thin film absorption spectrum of the acceptor molecule ABSeP-S.
[0037] Figure 7 This is the thin film absorption spectrum of the acceptor molecule ABQP-S.
[0038] Figure 8 J–V characteristic curves with PBDB-T as donor and ABTP-S and ABNP-S as acceptors.
[0039] Fig. 9 EQE characteristic curve with PBDB-T as donor and ABTP-S and ABNP-S as acceptors.
[0040] Fig.10 The J–V characteristic curves of the stacked cells prepared with PM6:Y6-O / BZ4F-O-1 and PBDB-T:ABTP-S / ABNP-S as front cells and PTTzF:Y6:
[70] PCBM as back cells, respectively.
[0041] Fig.11 J–V characteristic curves of single junction devices based on PM6:Y6-O / BZ4F-O-1 and PBDB-T:ABTP-S / ABNP-S under indoor lighting conditions. DETAILED DESCRIPTION
[0042] In order to make the purpose, technical solution and advantages of the present invention more clear, the specific implementation of the present invention is further described below with reference to the accompanying drawings and examples, but the implementation and protection of the present invention are not limited thereto. It should be pointed out that if there are processes that are not particularly described in detail below, they can be implemented or understood by those skilled in the art with reference to the prior art.
[0043] The practice of the present invention can adopt conventional techniques of organic synthetic chemistry and organic photovoltaic device preparation. In the following examples, efforts are made to ensure the accuracy of the numbers used (including mass, temperature, time, etc.), but some experimental errors and deviations should be considered. The temperatures used in the following examples are expressed in ° C, and the pressure is atmospheric pressure or near atmospheric pressure. The solvents used are analytically pure or chromatographically pure, all reactions are carried out in an inert gas atmosphere, and the device preparation is carried out in a nitrogen glove box. Unless otherwise indicated, all reagents are obtained through commercial channels.
[0044] Example 1
[0045]
[0046] (1) Raw materials or intermediate reactants
[0047] Triphenylphosphine (PPh3), tetrakistriphenylphosphine palladium (Pd(PPh3)4), 5-(bromomethyl)heptane, potassium carbonate (K2CO3), potassium iodide (KI), pyridine, N,N-dimethylformamide (DMF), 1,2-dichloroethane, tetrahydrofuran (THF), toluene, 1,2-dichlorobenzene, and chloroform were purchased from companies such as Anage, Bailingwei, and Suzhou Nakai.
[0048] (2) Preparation of Compound 4
[0049] Compound 1 (4,7-dibromo-5,6-dinitrobenzo[c][1,2,5]thiadiazole) (3.82 g, 10 mmol), compound 2 (6.02 g, 12 mmol), compound 3 (7.03 g, 12 mmol), Pd(PPh3)4 (346.2 mg, 0.3 mmol) were added to a toluene (60 mL) solution under nitrogen. The reaction mixture was heated to reflux and stirred for 12 h. After the reaction solution was cooled to room temperature, the reaction was quenched with water and extracted with dichloromethane. The organic phase was concentrated under reduced pressure to obtain a crude product, which was further purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as an eluent (V / V=2:1) to obtain compound 4 (the product was a red solid of 2.18 g, yield=29.8%).
[0050] (3) Synthesis of Compound 5
[0051] Under nitrogen atmosphere, compound 4 (1.46 g, 2 mmol) and PPh3 (5.24 g, 20 mmol) were added to 20 mL of o-dichlorobenzene (o-DCB). The reaction system was heated to 160 ° C and refluxed for 16 h. After the reaction was completed, it was cooled to room temperature, the solvent was removed by vacuum distillation, and 100 mL of methanol was used for precipitation. The crude product was filtered and used directly in the next step. The crude product, 5-(bromomethyl)heptane (1.78 g, 10 mmol), KI (0.55 g, 3.33 mmol), and K2CO3 (1.92 g, 12.92 mmol) were added to 50 mL of DMF. Under nitrogen conditions, the reaction was stirred at 80 ° C for 24 h. After cooling to room temperature, water was added and extracted three times with dichloromethane. The combined organic phase was further washed with water, dried with MgSO4, filtered and concentrated under reduced pressure. The product was purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as eluent (V / V=4:1) to obtain compound 5 (yellow oily liquid 0.93 g, yield = 52.2%).
[0052] (4) Synthesis of Compound 6
[0053] In a nitrogen atmosphere, POCl3 (3.06 g, 20 mmol) was slowly added to ultra-dry DMF (1.1 g, 15 mmol) at 0°C and reacted for 2 h. 25 mL of 1,2-dichloroethane containing compound 5 (0.89 g, 1 mmol) was slowly added dropwise to the reaction solution, reacted at 0°C for 1 h, and then heated to 90°C for 12 h. After the reaction was completed, it was cooled to room temperature and extracted with dichloromethane three times. The organic phase was dried over anhydrous MgSO4, filtered and the organic solvent was removed to obtain a crude product. The mixture was separated by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=1:2) to obtain compound 6 (0.83 g yellow solid, yield=87.7%).
[0054] (5) Compound ABTP-S
[0055] Under nitrogen atmosphere, compound 6 (300 mg, 0.317 mmol), compound 7 (300 mg, 1.5 mmol), and 30 mL of chloroform were added to a 100 mL two-necked flask, and 1 mL of pyridine was added, and the mixture was stirred at 65°C for 12 h. After the reaction solution was cooled to room temperature, methanol was used for precipitation, and the precipitate was collected by filtration. The crude product was separated by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=1:1) to obtain ABTP-S (353.5 mg of black solid, yield=85.2%).
[0056] Example 2
[0057]
[0058] (1) Raw materials or intermediate reactants
[0059] Triphenylphosphine (PPh3), tetrakistriphenylphosphine palladium (Pd(PPh3)4), 5-(bromomethyl)heptane, potassium carbonate (K2CO3), potassium iodide (KI), pyridine, N,N-dimethylformamide (DMF), 1,2-dichloroethane, tetrahydrofuran (THF), toluene, 1,2-dichlorobenzene, and chloroform were purchased from companies such as Anage, Bailingwei, and Suzhou Nakai.
[0060] (2) The preparation of compound 4, compound 5 and compound 6 is the same as that of ABTP-S.
[0061] (3) Compound ABTP-SCl
[0062] Under nitrogen atmosphere, compound 6 (300 mg, 0.317 mmol), compound 8 (350 mg, 1.5 mmol), and 30 mL of chloroform were added to a 100 mL two-necked flask, and 1 mL of pyridine was added, and the mixture was stirred at 65°C for 12 h. After the reaction solution was cooled to room temperature, methanol was used for precipitation, and the precipitate was collected by filtration. The crude product was separated by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=1:1) to obtain ABTP-SCl (384.6 mg of black solid, yield=83.2%).
[0063] Example 3
[0064]
[0065] (1) Raw materials or intermediate reactants
[0066] Triphenylphosphine (PPh3), tetrakistriphenylphosphine palladium (Pd(PPh3)4), 5-(bromomethyl)heptane, potassium carbonate (K2CO3), potassium iodide (KI), pyridine, N,N-dimethylformamide (DMF), 1,2-dichloroethane, tetrahydrofuran (THF), toluene, 1,2-dichlorobenzene, and chloroform were purchased from companies such as Anage, Bailingwei, and Suzhou Nakai.
[0067] (2) The preparation of compound 4, compound 5 and compound 6 is the same as that of ABTP-S.
[0068] (3) Compound ABTP-4Cl
[0069] Under nitrogen atmosphere, compound 6 (300 mg, 0.317 mmol), compound 9 (423 mg, 1.5 mmol), and 30 mL of chloroform were added to a 100 mL two-necked flask, and 1 mL of pyridine was added, and the mixture was stirred at 65°C for 12 h. After the reaction solution was cooled to room temperature, methanol was used for precipitation, and the precipitate was collected by filtration. The crude product was separated by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=2:1) to obtain ABTP-4Cl (379.4 mg of black solid, yield=81.2%).
[0070] Example 4
[0071]
[0072] (1) Raw materials or intermediate reactants
[0073] Triphenylphosphine (PPh3), tetrakistriphenylphosphine palladium (Pd(PPh3)4), 5-(bromomethyl)heptane, potassium carbonate (K2CO3), potassium iodide (KI), pyridine, N,N-dimethylformamide (DMF), 1,2-dichloroethane, tetrahydrofuran (THF), toluene, 1,2-dichlorobenzene, and chloroform were purchased from companies such as Anage, Bailingwei, and Suzhou Nakai.
[0074] (2) The preparation of compound 4, compound 5 and compound 6 is the same as that of ABTP-S.
[0075] (3) Compound ABTP-4F
[0076] Under nitrogen atmosphere, compound 6 (300 mg, 0.317 mmol), compound 10 (327 mg, 1.5 mmol), and 30 mL of chloroform were added to a 100 mL two-necked flask, and 1 mL of pyridine was added, and the mixture was stirred at 65°C for 12 h. After the reaction solution was cooled to room temperature, methanol was used for precipitation, and the precipitate was collected by filtration. The crude product was separated by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=2:1) to obtain ABTP-4F (352.4 mg of black solid, yield=82.6%).
[0077] Example 5
[0078]
[0079] (1) Raw materials or intermediate reactants
[0080] Triphenylphosphine (PPh3), tetrakistriphenylphosphine palladium (Pd(PPh3)4), 5-(bromomethyl)heptane, potassium carbonate (K2CO3), potassium iodide (KI), pyridine, N,N-dimethylformamide (DMF), 1,2-dichloroethane, tetrahydrofuran (THF), toluene, 1,2-dichlorobenzene, and chloroform were purchased from companies such as Anage, Bailingwei, and Suzhou Nakai.
[0081] (2) Preparation of Compound 12
[0082] Compound 11 (4,7-dibromo-2-(2-ethylhexyl)-5,6-dinitro-2H-benzo[D][1,2,3]triazole) (4.77 g, 10 mmol), compound 2 (6.02 g, 12 mmol), compound 3 (7.03 g, 12 mmol) and Pd(PPh3)4 (346.2 mg, 0.3 mmol) were added to a toluene (60 mL) solution under nitrogen. The reaction mixture was heated to reflux and stirred for 15 h. After the reaction solution was cooled to room temperature, the reaction was quenched with water and extracted with dichloromethane. The organic phase was concentrated under reduced pressure to obtain a crude product, which was further purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as an eluent (V / V=2:1) to obtain compound 12 (the product was a red solid of 2.17 g, yield=26.3%).
[0083] (3) Synthesis of Compound 13
[0084] Under nitrogen atmosphere, compound 12 (1.65 g, 2 mmol), PPh3 (5.24 g, 20 mmol) were added to 20 mL o-dichlorobenzene (o-DCB). The reaction system was heated to 160 ° C and refluxed for 16 h. After the reaction was completed, it was cooled to room temperature. The solvent was removed by distillation under reduced pressure and precipitated with 100 mL of methanol. The crude product was filtered and used directly in the next step. The crude product, 5-(bromomethyl)heptane (1.78 g, 10 mmol), KI (0.55 g, 3.33 mmol), K2CO3 (1.92 g, 12.92 mmol) were added to 50 mL of DMF. Under nitrogen conditions, the reaction was stirred at 80 ° C for 24 h. After cooling to room temperature, water was added and extracted three times with dichloromethane. The combined organic phase was further washed with water, dried with MgSO4, filtered and concentrated under reduced pressure. The product was purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as eluent (V / V=3:1) to obtain compound 13 (yellow oily liquid 0.87 g, yield = 44.3%).
[0085] (4) Synthesis of Compound 14
[0086] In a nitrogen atmosphere, POCl3 (3.06 g, 20 mmol) was slowly added to ultra-dry DMF (1.1 g, 15 mmol) at 0°C and reacted for 2 h. 25 mL of 1,2-dichloroethane containing compound 13 (0.98 g, 1 mmol) was slowly added dropwise to the reaction solution, reacted at 0°C for 1 h, and then heated to 90°C for 12 h. After the reaction was completed, the system was cooled to room temperature and extracted with dichloromethane three times. The organic phase was dried over anhydrous MgSO4, filtered and the organic solvent was removed to obtain a crude product. Compound 14 (0.87 g yellow solid, yield = 83.7%) was obtained by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V = 1:2).
[0087] (5) Compound ABNP-S
[0088] Under nitrogen atmosphere, compound 14 (300 mg, 0.288 mmol), compound 7 (280 mg, 1.4 mmol), and 30 mL of chloroform were added to a 100 mL two-necked flask, and 1 mL of pyridine was added, and the mixture was stirred at 65°C for 12 h. After the reaction solution was cooled to room temperature, methanol was used for precipitation, and the precipitate was collected by filtration. The crude product was separated by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=1:1) to obtain ABNP-S (333.1 mg of black solid, yield=82.3%).
[0089] Example 6
[0090]
[0091] (1) Raw materials or intermediate reactants
[0092] Triphenylphosphine (PPh3), tetrakistriphenylphosphine palladium (Pd(PPh3)4), 5-(bromomethyl)heptane, potassium carbonate (K2CO3), potassium iodide (KI), pyridine, N,N-dimethylformamide (DMF), 1,2-dichloroethane, tetrahydrofuran (THF), toluene, 1,2-dichlorobenzene, and chloroform were purchased from companies such as Anage, Bailingwei, and Suzhou Nakai.
[0093] (2) Preparation of Compound 16
[0094] Compound 15 (4,7-dibromo-5,6-dinitrobenzo[c][1,2,5]selenadiazole) (4.30 g, 10 mmol), compound 2 (6.02 g, 12 mmol), compound 3 (7.03 g, 12 mmol), Pd(PPh3)4 (346.2 mg, 0.3 mmol) were added to a toluene (60 mL) solution under nitrogen. The reaction mixture was heated to reflux and stirred for 12 h. After the reaction solution was cooled to room temperature, the reaction was quenched with water and extracted with dichloromethane. The organic phase was concentrated under reduced pressure to obtain a crude product, which was further purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as an eluent (V / V=2:1) to obtain compound 16 (the product was a red solid of 2.14 g, yield=27.5%).
[0095] (3) Synthesis of Compound 17
[0096] Under nitrogen atmosphere, compound 16 (1.56 g, 2 mmol) and PPh3 (5.24 g, 20 mmol) were added to 20 mL o-dichlorobenzene (o-DCB). The reaction system was heated to 160 ° C and refluxed for 16 h. After the reaction was completed, the system was cooled to room temperature, the solvent was removed by vacuum distillation, and 100 mL of methanol was used for precipitation. The crude product was filtered and used directly in the next step. The crude product, 5-(bromomethyl)heptane (1.78 g, 10 mmol), KI (0.55 g, 3.33 mmol), and K2CO3 (1.92 g, 12.92 mmol) were added to 50 mL DMF. Under nitrogen conditions, the reaction was stirred at 80 ° C for 24 h. After cooling to room temperature, water was added and extracted three times with dichloromethane. The combined organic phases were further washed with water, dried with MgSO4, filtered and concentrated under reduced pressure. The product was purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as eluent (V / V=3:1) to obtain compound 17 (yellow oily liquid 0.94 g, yield = 50.2%).
[0097] (4) Synthesis of Compound 18
[0098] In a nitrogen atmosphere, POCl3 (3.06 g, 20 mmol) was slowly added to ultra-dry DMF (1.1 g, 15 mmol) at 0°C and reacted for 2 h. 25 mL of 1,2-dichloroethane containing compound 5 (0.94 g, 1 mmol) was slowly added dropwise to the reaction solution, reacted at 0°C for 1 h, and then heated to 90°C for 12 h. After the reaction was completed, it was cooled to room temperature and extracted with dichloromethane three times. The organic phase was dried over anhydrous MgSO4, filtered and the organic solvent was removed to obtain a crude product. The mixture was separated by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=1:2) to obtain compound 18 (0.84 g yellow solid, yield=84.6%).
[0099] (5) Compound ABSeP-S
[0100] Under nitrogen atmosphere, compound 18 (300 mg, 0.302 mmol), compound 7 (300 mg, 1.5 mmol), and 30 mL of chloroform were added to a 100 mL two-necked flask, and 1 mL of pyridine was added, and the mixture was stirred at 65°C for 12 h. After the reaction solution was cooled to room temperature, methanol was used for precipitation, and the precipitate was collected by filtration. The crude product was separated by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=1:1) to obtain ABSeP-S (329.0 mg of black solid, yield=80.2%).
[0101] Example 7
[0102]
[0103] (1) Raw materials or intermediate reactants
[0104] Triphenylphosphine (PPh3), tetrakistriphenylphosphine palladium (Pd(PPh3)4), 5-(bromomethyl)heptane, potassium carbonate (K2CO3), potassium iodide (KI), pyridine, N,N-dimethylformamide (DMF), 1,2-dichloroethane, tetrahydrofuran (THF), toluene, 1,2-dichlorobenzene, and chloroform were purchased from companies such as Anage, Bailingwei, and Suzhou Nakai.
[0105] (2) Preparation of Compound 20
[0106] Compound 19 (5,8-dibromo-6,7-dinitroquinoxaline) (3.76 g, 10 mmol), compound 2 (6.02 g, 12 mmol), compound 3 (7.03 g, 12 mmol), Pd(PPh3)4 (346.2 mg, 0.3 mmol) were added to a toluene (60 mL) solution under nitrogen. The reaction mixture was heated to reflux and stirred for 12 h. The reaction solution was cooled to room temperature, quenched with water, and extracted with dichloromethane. The organic phase was concentrated under reduced pressure to obtain a crude product, which was further purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as an eluent (V / V=3:2) to obtain compound 20 (the product was a red solid of 1.62 g, yield=22.4%).
[0107] (3) Synthesis of Compound 21
[0108] Under nitrogen atmosphere, compound 20 (1.45 g, 2 mmol) and PPh3 (5.24 g, 20 mmol) were added to 20 mL of o-dichlorobenzene (o-DCB). The reaction system was heated to 160 ° C and refluxed for 16 h. After the reaction was completed, it was cooled to room temperature, the solvent was removed by vacuum distillation, and 100 mL of methanol was used for precipitation. The crude product was filtered and used directly in the next step. The crude product, 5-(bromomethyl)heptane (1.78 g, 10 mmol), KI (0.55 g, 3.33 mmol), and K2CO3 (1.92 g, 12.92 mmol) were added to 50 mL of DMF. Under nitrogen conditions, the reaction was stirred at 80 ° C for 24 h. After cooling to room temperature, water was added and extracted three times with dichloromethane. The combined organic phases were further washed with water, and the organic phases were dried with MgSO4, filtered and concentrated under reduced pressure. The product was purified by silica gel column chromatography using a mixed solvent of petroleum ether and dichloromethane as eluent (V / V=4:1) to obtain compound 21 (yellow oily liquid 0.85 g, yield = 48.3%).
[0109] (4) Synthesis of Compound 22
[0110] In a nitrogen atmosphere, POCl3 (3.06 g, 20 mmol) was slowly added to ultra-dry DMF (1.1 g, 15 mmol) at 0°C and reacted for 2 h. 25 mL of 1,2-dichloroethane containing compound 21 (0.88 g, 1 mmol) was slowly added dropwise to the reaction solution, reacted at 0°C for 1 h, and then heated to 90°C for 12 h. After the reaction was completed, it was cooled to room temperature and extracted with dichloromethane three times. The organic phase was dried over anhydrous MgSO4, filtered and the organic solvent was removed to obtain a crude product. The mixture was separated by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=1:1) to obtain compound 22 (0.78 g yellow solid, yield=83.5%).
[0111] (5) Compound ABQP-S
[0112] Under nitrogen atmosphere, compound 22 (300 mg, 0.319 mmol), compound 7 (320 mg, 1.6 mmol), and 30 mL of chloroform were added to a 100 mL two-necked flask, and 1 mL of pyridine was added, and the mixture was stirred at 65°C for 12 h. After the reaction solution was cooled to room temperature, methanol was used for precipitation, and the precipitate was collected by filtration. The crude product was separated by column chromatography using a mixed solvent of petroleum ether and dichloromethane as the eluent (V / V=1:1) to obtain ABQP-S (340 mg of black solid, yield=81.7%).
[0113] Figure 1 This is the UV-visible absorption spectrum of the compound ABTP-S film. In the range of 300-900 nm, the absorption peak of the compound ABTP-S is located at 705 nm, the optical absorption edge is 740 nm, and the corresponding optical band gap is 1.68 eV.
[0114] Figure 2 This is the UV-visible absorption spectrum of the compound ABTP-SCl film. In the range of 300-900 nm, the absorption peak of the compound ABTP-SCl is located at 713 nm, the optical absorption edge is 750 nm, and the corresponding optical band gap is 1.65 eV.
[0115] Figure 3 This is the UV-visible absorption spectrum of the compound ABTP-4Cl film. In the range of 300-900 nm, the absorption peak of the compound ABTP-4Cl is located at 686 nm, the optical absorption edge is 735 nm, and the corresponding optical band gap is 1.69 eV.
[0116] Figure 4This is the UV-visible absorption spectrum of the compound ABTP-4F film. In the range of 300-900 nm, the absorption peak of the compound ABTP-4F is located at 696 nm, the optical absorption edge is 725 nm, and the corresponding optical band gap is 1.71 eV.
[0117] Figure 5 This is the UV-visible absorption spectrum of the compound ABNP-S film. In the range of 300-900 nm, the absorption peak of the compound ABNP-S is located at 715 nm, while the optical absorption edge is 765 nm, and the corresponding optical band gap is 1.62 eV.
[0118] Figure 6 This is the UV-visible absorption spectrum of the compound ABSeP-S film. In the range of 300-900nm, the absorption peak of the compound ABSeP-S is located at 717nm, the optical absorption edge is 750nm, and the corresponding optical band gap is 1.65eV.
[0119] Figure 7 This is the UV-visible absorption spectrum of the compound ABQP-S film. In the range of 300-900nm, the absorption peak of the compound ABQP-S is located at 697nm, the optical absorption edge is 730nm, and the corresponding optical band gap is 1.70eV.
[0120] Figure 8 JV curves of organic solar cell devices based on PBDB-T:ABTP-S and PBDB-T:ABNP-S. The PBDB-T:ABTP-S device exhibited an open circuit voltage of 1.10 volts, a short circuit current of 16.95 mA / cm2, and a fill factor of 78.03%. Finally, an efficiency of 14.55% was achieved. The PBDB-T:ABNP-S device exhibited an open circuit voltage of 1.08 volts, a short circuit current of 17.24 mA / cm2, and a fill factor of 77.28%. Finally, an efficiency of 14.39% was achieved.
[0121] Fig. 9 The following are the EQE curves of organic solar cell devices based on PBDB-T:ABTP-S and PBDB-T:ABNP-S. It can be found that both devices have good light response in the 300-740nm spectral range. The EQE of the PBDB-T:ABTP-S device in the 400-690nm range exceeds 70%, while the EQE of the PBDB-T:ABNP-S device in the 400-700nm range exceeds 70%. Therefore, both devices show excellent performance.
[0122] Fig.10The J–V characteristic curves of stacked cells prepared with PM6:Y6-O / BZ4F-O-1 and PBDB-T:ABTP-S / ABNP-S as front cells and PTTzF:Y6:
[70] PCBM as back cells were shown. The PM6:Y6-O device exhibited an open circuit voltage of 1.75 V, a short circuit current of 14.30 mA / cm2, and a fill factor of 77.25%. Finally, an efficiency of 19.33% was achieved. The PM6:BZ4F-O-1 device exhibited an open circuit voltage of 1.74 V, a short circuit current of 14.10 mA / cm2, and a fill factor of 74.89%. Finally, an efficiency of 18.37% was achieved. The PBDB-T:ABTP-S device exhibited an open circuit voltage of 1.92 V, a short circuit current of 13.86 mA / cm2, and a fill factor of 78.12%. Finally, an efficiency of 20.79% was achieved. The PBDB-T:ABNP-S device exhibited an open-circuit voltage of 1.90 V and a short-circuit current of 13.85 mA / cm2 with a fill factor of 77.00%. The final efficiency was 20.26%.
[0123] Fig.11 The J–V characteristic curves of single-junction cells with PM6:Y6-O / BZ4F-O-1 and PBDB-T:ABTP-S / ABNP-S as active layers under indoor lighting conditions are shown. The PM6:Y6-O device exhibits an open circuit voltage of 0.86 V, a short circuit current of 126.32 μA / cm2, and a fill factor of 80.02%. Finally, an efficiency of 30.61% was achieved. The PM6:BZ4F-O-1 device exhibits an open circuit voltage of 0.79 V, a short circuit current of 123.87 μA / cm2, and a fill factor of 75.37%. Finally, an efficiency of 25.97% was achieved. The PBDB-T:ABTP-S device exhibits an open circuit voltage of 0.97 V, a short circuit current of 119.76 μA / cm2, and a fill factor of 79.26%. Finally, an efficiency of 32.42% was achieved. The PBDB-T:ABNP-S device exhibited an open-circuit voltage of 0.95 V and a short-circuit current of 122.39 μA / cm2 with a fill factor of 74.28%. The final efficiency was 30.41%.
[0124] Example 8
[0125] The materials obtained in Examples 1 and 5 (ABTP-S, ABNP-S) are used as examples to illustrate the application of the asymmetric medium bandgap fused ring acceptor materials in the present invention in organic solar cells and indoor photovoltaic devices, but the present invention is not limited to the examples given.
[0126] The specific preparation process of the device is as follows:
[0127] (1) Single junction device preparation
[0128] A 40nm hole transport layer (PEDOT:PSS) was spin-coated on the ITO glass, followed by a 100nm photoactive layer of the donor and acceptor materials, and then a 5nm PFN-Br layer was spin-coated as the cathode interface layer, and then a 100nm Ag electrode was evaporated to complete the device preparation. The device was then tested under a standard solar simulator and an indoor light simulator.
[0129] (2) Preparation of stacked devices
[0130] The stacked device adopts the following structure: ITO / PEDOT:PSS / front cell active layer / connection layer / rear cell active layer / PDINO / Ag. The preparation process of the front cell active layer is the same as that of the single-cell device. Preparation of the connection layer (ZnO / PEDOT:PSS / PMA): First, a ZnO nanoparticle layer (about 20nm) is spin-coated on the active layer of the front cell, and then PEDOT:PSS (diluted with deionized water at a ratio of 1:2.5) is spin-coated on the ZnO layer (about 15nm). The substrate is thermally annealed at 100℃ for 5min, and then about 5nm of phosphomolybdic acid (PMA) is spin-coated on PEDOT:PSS. The preparation method of the rear cell active layer is the same as that of the single-cell device. After the front cell, connection layer and rear cell active layer are prepared, the electron transport layer PDINO is spin-coated (3000rpm). Finally, the Ag electrode is deposited by evaporation under high vacuum to obtain a stacked cell device.
[0131] Table 1. Device performance parameters of ITO / PEDOT:PSS / PBDB-T:Acceptor / PFN-Br / Ag (AM1.5G)
[0132]
[0133] Table 2. Performance parameters of stacked solar cell devices prepared with ITO / PEDOT:PSS / PBDB-T:acceptor / PFN-Br / Ag as the front cell and ITO / PEDOT:PSS / PTTzF:Y6:
[70] PCBM / PDINO / Ag as the back cell (AM1.5G)
[0134]
[0135] Table 3. Performance parameters of tandem solar cell devices obtained by using ITO / PEDOT:PSS / PBDB-T:ABTP-S / PFN-Br / Ag as the front cell, PTTzF:Y6:
[70] PCBM, PTB7-Th:O6T-4F and PM6:BTP-eC9 as the back cell, and the device structure is ITO / PEDOT:PSS / active layer / PDINO / Ag as the back cell (AM1.5G)
[0136]
[0137] Table 4. Performance parameters of ITO / PEDOT:PSS / PBDB-T:Acceptor / PFN-Br / Ag devices under indoor lighting (1000 Lux, input power (P in ) is 284 microwatts per square centimeter)
[0138]
[0139] As shown in Table 1, the single junction devices prepared with PBDB-T as the donor and ABTP-S and ABNP-S as the acceptors all exhibited an open circuit voltage close to 1.1 V, a high fill factor, and good device efficiency. The corresponding JV curves and EQE curves are shown in the attached Figure 8 and 9 , which shows that this type of material has great application potential. The front cells were prepared with PBDB-T:ABTP-S and PBDB-T:ABNP-S as the active layer, and the back cells were prepared with PTTzF:Y6:
[70] PCBM as the active layer. The performance of the tandem solar cell device is shown in Table 2. Since the medium-bandgap material and the narrow-bandgap material have good complementary absorption, and the front cell has excellent photovoltaic performance, the efficiency of the above-mentioned tandem solar cell devices exceeds 20%. In particular, the efficiency of the tandem cell device based on ABTP-S reached 20.79%. In addition, in order to study the universality of medium-bandgap materials in tandem cells, the front cell with PBDB-T:ABTP-S as the active layer was matched with different back cells, and the device data are shown in Table 3. It can be found that the precell based on the medium bandgap acceptor not only matches well with PTTzF:Y6:
[70] PCBM, but also achieves 17.54% and 20.21% efficiency in the stacked device with PTB7-Th:O6T-4F and PM6:BTP-eC9, respectively. The above results show that the medium bandgap acceptor material in the present invention not only exhibits good device efficiency in single junction devices, but also has excellent performance and universality in stacked cell devices, which indicates that the asymmetric medium bandgap acceptor is a class of highly promising precell materials.
[0140] The absorption spectra of the medium bandgap acceptor ABTP-S and ABNP-S devices are very consistent with the luminescence spectra of indoor light sources, so single junction devices of PBDB-T:ABTP-S and PBDB-T:ABNP-S were prepared, and the device performance obtained under indoor lighting conditions is shown in Table 4. The devices based on ABTP-S and ABNP-S showed excellent device efficiencies of 32.42% and 31.63%, respectively. This result shows that the medium bandgap acceptor in the present invention has a good application in the field of indoor photovoltaics.
[0141] Comparative Example
[0142]
[0143] In order to further illustrate that the asymmetric medium band gap receptor involved in the present invention has unique advantages in OSCs, taking the embodiments ABTP-S and ABNP-S involved in the present invention as examples, receptors with similar structures and symmetrical structures are selected for comparison (Comparative Example 1 and Comparative Example 2). Both Y6-O and BZ4F-O-1 contain alkoxy side chains and strong electron-withdrawing end groups. The difference is that Y6-O is a symmetrical seven-ring receptor with benzothiadiazole as the core unit, which forms a sharp contrast with the ABTP-S molecule in terms of molecular symmetry. BZ4F-O-1 is a symmetrical five-ring receptor with benzotriazole as the core, which forms a sharp contrast with the ABNP-S molecule in terms of molecular symmetry. Under the same conditions, single-junction devices and stacked devices were prepared using the above four materials as receptors, and the single-junction devices were tested under standard sunlight and indoor light environments, respectively. The relevant device data are shown in Tables 5-7.
[0144] Table 5. Device parameters of single-junction organic solar cells based on PM6:Y6-O / BZ4F-O-1 and PBDB-T:ABTP-S / ABNP-S under standard sunlight conditions (AM1.5G)
[0145]
[0146] It can be found from the single junction device data (Table 5) that compared with Comparative Examples 1 and 2, due to the use of weak electron-withdrawing end groups in ABTP-S and ABNP-S, more excellent medium band gap absorption and high LUMO energy levels are exhibited, so the open circuit voltage of the devices based on ABTP-S and ABNP-S is also significantly improved. Not only that, the presence of the asymmetric structure can promote charge transfer and reduce material crystallization. The fill factor of the devices based on ABTP-S and ABNP-S is improved. Finally, the devices based on ABTP-S and ABNP-S exhibit high open circuit voltage and good device performance.
[0147] Table 6. Device parameters of tandem organic solar cells prepared with PM6:Y6-O / BZ4F-O-1 and PBDB-T:ABTP-S / ABNP-S as front cells and PTTzF:Y6:
[70] PCBM as back cells under standard sunlight conditions (AM1.5G)
[0148]
[0149] Front cells were prepared using ABTP-S, ABNP-S and two comparative materials as acceptors, and back cells were prepared using PTTzF:Y6:
[70] PCBM as the active layer to obtain stacked solar cell devices. The device performance is shown in Table 6. Since the single junction device of PBDB-T:ABTP-S / ABNP-S has a higher open circuit voltage than the PM6:Y6-O / BZ4F-O-1 device, the open circuit voltage of the stacked device based on ABTP-S and ABNP-S is significantly higher than that of the two comparative materials. Since the fill factor of the device of comparative example 2 is low, the fill factor of the stacked device is limited, so the device efficiency is only 18.37%. Thanks to the high open circuit voltage and better device performance of the PBDB-T:ABTP-S / ABNP-S device, the stacked device based on ABTP-S and ABNP-S achieved device efficiencies of 20.79% and 20.26%, which are higher than the two comparative examples. This further illustrates that the medium bandgap asymmetric acceptor reported in the present invention is a good front cell material.
[0150] Table 7. Device parameters of single junction devices based on PM6:Y6-O / BZ4F-O-1 and PBDB-T:ABTP-S / ABNP-S under indoor light conditions (1000Lux, input power (P in ) is 284 microwatts per square centimeter).
[0151]
[0152] The device performance of the single junction devices based on the above four acceptor materials under indoor lighting conditions is shown in Table 7. Due to the high LUMO energy levels of ABTP-S and ABNP-S, the device based on PBDB-T:ABTP-S / ABNP-S exhibits a higher open circuit voltage than the PM6:Y6-O / BZ4F-O-1 device. In addition, due to the characteristics of the asymmetric structure that promotes charge transfer and reduces material crystallization. Therefore, the devices based on ABTP-S and ABNP-S exhibit good short-circuit current and fill factor. Finally, the device based on PBDB-T:ABTP-S obtained the best device efficiency of 32.42% under indoor lighting.
[0153] The above embodiments of the present invention are only examples for clearly illustrating the present invention, and are not intended to limit the embodiments of the present invention. For those skilled in the art, other different forms of changes or modifications can be made based on the above description. It is not necessary and impossible to list all the embodiments here. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention should be included in the protection scope of the claims of the present invention.
Claims
1. A class of asymmetric medium band gap fused ring receptor materials, the general structural formula of which is shown in Formula I: in: R in the structural formula 1 , R 2 , R 3 are independently selected from linear, branched or alkyl-substituted aryl side chains having 1 to 40 carbon atoms; The Weak A unit is selected from any one of the following structural formulas: in: The dotted line in the Weak A structure indicates the connection site to the Weak A unit.
2. According to the asymmetric medium band gap fused ring receptor material of claim 1, Ar 1 The unit is selected from any one of the following structural formulas: in, Ar 1 R in the structural formula 4 are independently selected from H, a linear or branched alkyl group having 1 to 20 carbon atoms, wherein Ar 1 The dashed lines in the structural formula indicate the connection sites to other units.
3. A method for preparing a class of asymmetric medium band gap fused ring receptor materials according to claim 1 or 2, The following steps are involved: Its synthetic route is as follows: R in the structural formula 1 , R 2 , R 3 Each is independently selected from a linear, branched or alkyl-substituted aryl side chain having 1 to 40 carbon atoms.
4. The preparation method according to claim 3, It is characterized in that The steps include: (1) Compound A, Compound B and Compound C are added to 80-100 mL of toluene, and then a catalyst tetrakis(triphenylphosphine)palladium is added; and a compound D is obtained through a Stille coupling reaction; (2) Under nitrogen protection, compound D and triphenylphosphine are added to o-dichlorobenzene, and then the system is heated to react to obtain compound E; (3) Under nitrogen protection, compound E and halogenated alkane R 3 Br, potassium carbonate and potassium iodide are added to N,N-dimethylformamide to react to obtain compound F; (4) This reaction is a Vilsmeier-Haack reaction. Compound F is dissolved in 1,2-dichloroethane and then added dropwise to the formylation reagent phosphorus oxychloride at -10 to 0°C. After reacting at low temperature for 1 to 2 hours, the system is heated to 80 to 100°C and reacted for 8 to 12 hours to obtain compound G. (5) This reaction is a Knoevenagel condensation reaction. Under nitrogen protection, compound G is reacted with Weak A and pyridine to obtain compound H.
5. The preparation method according to claim 4, It is characterized in that In step (1), the reaction conditions of the Stille coupling reaction are: reacting at 80-90° C. for 10-12 h.
6. The preparation method according to claim 4, It is characterized in that In step (2), the reaction is carried out at 160-180° C. for 16-18 hours.
7. The preparation method according to claim 4, It is characterized in that In step (3), the reaction is carried out at 80-85° C. for 10-12 hours.
8. The preparation method according to claim 4, It is characterized in that In step (4), the molar ratio of compound F to phosphorus oxychloride is 1:10 to 1:
30.
9. The preparation method according to claim 4, It is characterized in that In step (5), the reaction is carried out at 60° C. for 5 to 8 hours.
10. The asymmetric medium bandgap fused ring acceptor material according to claim 1 or 2 is used in the field of stacked organic solar cells and indoor photovoltaic devices.
Citation Information
Patent Citations
Asymmetric fused heterocyclic small molecule electron acceptor material based on dithienopyrrole and application thereof
CN110577548A
3-alkylthiophene-based hepta-fused heterocyclic conjugated small molecule as well as preparation method and application thereof
CN110606856A
Condensed ring benzoselenadiazole non-fullerene acceptor material as well as preparation method and application thereof
CN111285885A
Diester thiophene non-fused ring electron acceptor material and preparation method and application thereof