Surface modification compound and preparation method thereof
The surface-modified compounds enable efficient and cost-effective protein grafting on various materials, enhancing Western Blot technology's applicability to diverse materials like quartz, PMMA, and PDMS, with improved signal detection.
Patent Information
- Application Number
- CN202410998936.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-07-24
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-07-24
AI Technical Summary
Existing methods for protein detection, such as Western Blot and Western Blot, are labor-intensive, costly, and time-consuming, limiting their application, especially for trace expression analysis of proteins.
A surface-modified compound and its preparation method, which includes a surface-modified compound and a preparation method thereof, which are used to prepare a surface-modified compound and a preparation method thereof, characterized by a chemical structure that reacts with a new surface-modified compound to form a stable chemical bond, so that the material has a protein grafting ability that would not otherwise be achieved.
The surface-modified compounds provide a simple, high-yield, and cost-effective method for protein grafting on various materials, expanding the applicability of Western Blot technology to different materials, including quartz, PMMA, and PDMS, with improved signal detection.
Smart Images

Figure CN119080821A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of surface modified compound preparation, in particular to a surface modified compound and a preparation method thereof. Background Art
[0002] Western Blot method is a kind of labor-intensive laboratory analysis method, and it is widely used in life science to determine whether there is target protein in complex sample and to determine the relative amount of target protein.Due to the need to use protein amount is large, complicated operation, reagent consumption is large, time-consuming and other deficiencies make its application limited, especially for the research of trace level expression protein there is obvious deficiency.So, Western Blot technology develops a variety of different implementation methods, wherein Simple Western is a kind of simple and practical method, it is generally used to study the expression level of trace protein, and its advantages are simple, fast, with low cost and scalability.In addition, due to not needing to use complicated chemiluminescence or fluorescence detection method, Simple Western is applicable to the expression level of studying trace protein, particularly for those protein samples that are difficult to prepare a large amount of standards.
[0003] The material surface grafting modification method can improve the properties of different materials by modifying and grafting different coupling agents on the material surface, so that its functionality can be expanded to different degrees. Applying this modification idea to different materials can realize the application of Simple Western on materials with different characteristics, greatly expanding its application area, which is of great significance for realizing Simple Western testing on different materials.
[0004] Benzophenone, as a commonly used photosensitive group, can generate highly active free radical intermediates under the excitation of light of a specific wavelength (generally ultraviolet rays around 365nm), which can quickly form covalent bonds with surrounding components such as amino acid molecules in proteins. The reaction formula is shown below. Combining this characteristic, surface-modified compounds can be prepared, making it possible to fix proteins on the surfaces of many materials.
[0005] Summary of the invention
[0006] In order to overcome the shortcomings and deficiencies of the prior art, the present invention provides a surface-modified compound and a preparation method thereof. The present invention performs surface modification on a variety of commonly used materials, such as quartz, PMMA, PDMS, etc., so that the surface reacts with a new surface-modified compound to form a stable chemical bond, so that the material has a protein grafting ability that would not otherwise be achieved. This type of new surface-modified compound synthesis process has the advantages of simple synthesis, high yield, good grafting effect, and low cost, providing more options and grafting ideas for subsequent material modification, expanding the synthesis ideas of surface modifiers, and providing more surface-modified compounds for selection.
[0007] The purpose of the present invention is achieved through the following technical solutions:
[0008] In a first aspect, the present invention provides a surface-modified compound, characterized in that the chemical structure is as shown in formula (I):
[0009]
[0010] Wherein R1 is selected from
[0011]
[0012] R2 is selected from H2 or CH3.
[0013] Furthermore, the surface modified compound is represented by formula (II), formula (III) or formula (IV):
[0014]
[0015] In a second aspect, the present invention provides a modified quartz plate, wherein the modified quartz plate is formed by grafting a pretreated quartz plate with a surface modification compound, and the chemical structure of the surface modification compound is as shown in formula (II) described in the first aspect.
[0016] In a third aspect, the present invention provides a method for preparing the modified quartz plate as described in the second aspect, wherein the preparation steps are as follows:
[0017] 1) Pre-treat the quartz plate;
[0018] 2) Grafting 3-aminopropyltrimethoxysilane onto quartz plate: prepare a mixed solution of 3-aminopropyltrimethoxysilane and methanol, add it into a square culture dish, immerse the quartz plate in the mixed solution, place the square culture dish in an oven for reaction, rinse with methanol, and finally blow dry with nitrogen for standby use.
[0019] 3) Connecting 3-(bromomethyl)benzophenone to 3-aminopropyltrimethoxysilane: using DMF to dissolve 3-(bromomethyl)benzophenone and potassium carbonate powder, after light protection and ultrasound, a mixed solution is formed; then the quartz plate treated in step 2) is immersed in the mixed solution, reacted at room temperature, and after the connection is completed, rinsed with DMF, then rinsed with PBST, and finally dried with nitrogen to obtain a modified quartz plate.
[0020] Furthermore, in step 1), the pretreatment refers to sequentially flushing the quartz plate with a 0.1 mol / L HCl solution for 30 min, then flushing with deionized water for 10 min, flushing the quartz plate with a 0.1 mol / L NaOH solution for 2 h, then flushing with methanol for 10 min, and finally drying with nitrogen.
[0021] Furthermore, in step 2), the reaction time is 12-16 hours.
[0022] The synthetic route of the modified quartz plate is:
[0023]
[0024] The present invention also provides another method for preparing the modified quartz plate as described in the second aspect, and the preparation steps are as follows:
[0025] 1) Synthesis of pheny l(3-(((3-(trimethoxys ilyl)propy l)amino)methy l)phenyl)-methanone (surface modified compound (II)): 3-aminopropyltrimethoxysilane (APS), 3-(bromomethyl)benzophenone and potassium carbonate were dissolved in DMF, protected from light, reacted at room temperature, and a white solid was precipitated. The solid was filtered, dried with water, rinsed with methanol, and dried to obtain a surface modified compound (II);
[0026] 2) Pre-treating the quartz plate;
[0027] 3) Connecting the surface modified compound (II) to the treated quartz plate: prepare a mixed solution of the surface modified compound (II) and DMF, add the solution into a square culture dish, immerse the quartz plate in the mixed solution until it is completely covered by the mixed solution, place the square culture dish in an oven for reaction, rinse after the connection is completed, and finally blow dry with nitrogen to obtain a modified quartz plate.
[0028] Further, in step 2), the pretreatment refers to sequentially flushing the quartz plate with a 0.1 mol / L HCl solution for 30 min, then flushing with deionized water for 10 min, flushing the quartz plate with a 0.1 mol / L NaOH solution for 2 h, then flushing with methanol for 10 min, and finally drying with nitrogen.
[0029] Another synthetic route of the modified quartz plate is:
[0030]
[0031] In a fourth aspect, the present invention provides a modified PDMS plate, wherein the modified PDMS plate is formed by grafting a surface modification compound onto a PDMS plate after hydrosilation treatment, wherein the chemical structure of the surface modification compound is as shown in formula (III) described in the first aspect.
[0032] In a fifth aspect, the present invention provides a method for preparing the modified PDMS plate as described in the fourth aspect, wherein the preparation steps are as follows:
[0033] 1) Synthesis of pent-4-en-1-yl 2-(3-benzoy l pheny l)propanoate (surface-modified compound (III)): Ketoprofen and 4-penten-1-ol were dissolved in DMF, DMAP was added and stirred, and then EDC 1 was added. The reaction was extracted at room temperature, and the mixture was spin-dried and purified to obtain the surface-modified compound (III).
[0034] 2) Place the PDMS-Si-H membrane into a dry isopropanol solution containing the surface modification compound (III). Use a quartz dropper to absorb the Karstedts Pt catalyst, add it to the reaction system after activation, mix well and react. After the reaction is completed, wash it several times and vacuum dry it to obtain a modified PDMS plate.
[0035] Furthermore, in step 2), the PDMS-Si-H membrane is a PDMS sheet whose surface is hydrogenated after being treated with dilute hydrochloric acid.
[0036] The synthetic route of the modified PDMS plate is:
[0037]
[0038] In a sixth aspect, the present invention provides a modified PMMA plate, wherein the modified PMMA plate is formed by grafting a PMMA plate after plasma cleaning with a surface modification compound, wherein the chemical structure of the surface modification compound is as shown in formula (IV) described in the first aspect.
[0039] In a seventh aspect, the present invention provides a method for preparing the modified PMMA plate as described in the sixth aspect, wherein the preparation steps are as follows:
[0040] 1) Synthesis of 2-(3-benzoy l pheny l)-N-(3-(triethoxys i ly l)propy l)propanamide (surface-modified compound (IV)): Ketoprofen and 3-aminopropyltrimethoxysilane were dissolved in DMF, DMAP was added and stirred, and then EDC 1 was added. The mixture was reacted at room temperature, extracted, spin-dried and purified to obtain a surface-modified compound (IV) in the form of a transparent oil.
[0041] 2) Clean the PMMA plate with a plasma cleaner, and immediately immerse it in a methanol alkaline solution of the surface modification compound (IV) obtained in step 1) to carry out grafting reaction overnight in the dark, and finally clean it with methanol to obtain a modified PMMA plate.
[0042] Furthermore, in step 2), the cleaning conditions of the plasma cleaning machine are as follows: time 120s, power 210W, and oxygen gas.
[0043] The synthetic route of the modified PMMA plate is:
[0044]
[0045] The parent nucleus of the present invention is benzophenone, which is a commonly used photosensitive group. The photosensitive group generates highly active intermediates under the excitation of light of a specific wavelength (generally ultraviolet rays near 365nm), and these intermediates can quickly form covalent bonds with amino acids in surrounding proteins, thereby achieving the purpose of grafting proteins. Due to the development of Western Blot technology, it is necessary to complete the grafting and fixation of proteins on the surfaces of different materials, and many materials (such as quartz, PMMA, PDMS, etc.) themselves cannot connect proteins. Therefore, the present invention develops 4 different grafting methods, using three different benzophenone derivatives to combine with different plate surfaces treated in different ways, to achieve surface protein grafting of multiple materials.
[0046] Compared with the existing technical solutions, the present invention has the following advantages:
[0047] 1. The three surface modification compounds of the present invention can be used as different materials for surface modification of grafted proteins according to the surface properties of the materials, which expands the range of selectable surface modification compounds and broadens the range of materials that can be used in the simple western method.
[0048] 2. The three surface-modified compounds of the present invention have the characteristics of low raw material cost, few synthesis steps, high synthesis yield, simple purification, good solubility, etc.
[0049] 3. The surface grafting concept of the present invention includes but is not limited to the surface grafting of quartz, PMMA, PDMS, capillaries and chips, and can be selected according to the scheme corresponding to the characteristics of the material itself, with high flexibility. BRIEF DESCRIPTION OF THE DRAWINGS
[0050] Figure 1 The signal test result diagram of Example 1 and Comparative Example 1;
[0051] Figure 2 The signal test result diagram of Example 2 and Comparative Example 2;
[0052] Figure 3 The signal test result diagram of Example 3 and Comparative Example 3;
[0053] Figure 4 It is a signal test result diagram of Example 4 and Comparative Example 4. DETAILED DESCRIPTION
[0054] The technical solutions in the embodiments are described clearly and completely below. Obviously, the embodiments described below are only some embodiments of the present invention, not all embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0055] It should be understood that when used in this specification and the appended claims, the terms "include" and "comprises" indicate the presence of described features, integers, steps, operations, elements and / or components, but do not exclude the presence or addition of one or more other features, integers, steps, operations, elements, components and / or combinations thereof.
[0056] It should also be understood that the terms used in this description of the embodiments of the present invention are only for the purpose of describing specific embodiments and are not intended to limit the embodiments of the present invention. As used in the description of the embodiments of the present invention and the appended claims, unless the context clearly indicates otherwise, the singular forms of "a", "an" and "the" are intended to include plural forms.
[0057] The raw materials involved in the present invention can be directly purchased from the market. For process parameters not specifically noted, conventional techniques can be used.
[0058] Example 1: Testing of modified quartz plates.
[0059] 1) Pretreatment of the quartz plate: rinse the quartz plate with 0.1 mol / L HCl solution for 30 min, then rinse with deionized water for 10 min, rinse the quartz plate with 0.1 mol / L NaOH solution for 2 h, then rinse with methanol for 10 min, and finally blow dry with nitrogen.
[0060] 2) Grafting 3-aminopropyltrimethoxysilane (APS) onto quartz plate: Prepare a mixed solution of 3-aminopropyltrimethoxysilane and methanol (volume ratio: V APS :V MeOH =1:1) 50mL, then pour it into a square culture dish, then immerse the quartz plate in the square culture dish until it is completely covered by the mixed solution, then place the square culture dish in a 37° oven to react for 12-16 hours to complete the APS connection, then rinse with methanol for 10 minutes, and finally blow dry with nitrogen for use.
[0061] 3) Connecting 3-(bromomethyl)benzophenone to 3-aminopropyltrimethoxysilane: Dissolve 55 mg of 3-(bromomethyl)benzophenone and 5 mg of potassium carbonate powder in 50 mL of DMF, and perform ultrasound in a dark environment for 2 hours. Then, immerse the quartz plate treated in step 2) in the mixed solution, and react at room temperature for 12-16 hours. After the connection is completed, rinse with DMF for 3 minutes, then rinse with PBST for 3 minutes, and finally blow dry with nitrogen for use.
[0062] 4) Protein solidification treatment: Use a pipette to take 3 μL of protein sample (HRP protein - concentration 10 ng / μL) and add it to five different positions on the surface of the quartz plate treated in step 3), then irradiate at a wavelength of 350 mm for more than 30 minutes. After irradiation, use PBST to rinse the surface of the quartz plate, and finally spread the ultra-sensitive ECL luminescent liquid on the surface of the quartz plate. Use the 6000pro II luminescent camera produced by Guangzhou Boluteng Biotechnology Co., Ltd. to record the protein fixation effect.
[0063] Comparative Example 1: Similarly, a pipette was used to draw 3uL of protein sample (HRP protein - concentration 10ng / μL) to five different positions on the surface of the quartz plate treated in step 3). The difference from the above is that Comparative Example 1 was not irradiated at a wavelength of 350mm, but was only placed in a dark environment (the placement time was consistent with the irradiation time in step 4)), and then PBST was used to rinse the surface of the quartz plate, and finally the ultrasensitive ECL luminescent liquid was spread all over the surface of the quartz plate, and 6000pro II was used to take photos and record the luminescence.
[0064] The photo recording results are shown in Table 1 and Figure 1 As shown, it can be seen from the experimental result diagram that there is an obvious difference in the results of signal detection after adding ECL luminescent liquid to the two modified quartz plates with and without irradiation after adding the protein sample. The average maximum signal of the five points of Example 1 treated with irradiation is about 20000 cts, while the average maximum signal of the five points of Control Example 1 not treated with irradiation is about 3500 cts. Therefore, the signal of Example 1 treated with irradiation is obviously greater than the signal of Control Example 1.
[0065] Table 1 Signal values of Example 1 and Comparative Example 1
[0066]
[0067] Example 2: Testing of modified quartz plate
[0068] 1)pheny l(3-(((3-(tr imethoxys ilyl)propy l)amino)methy l)pheny l)
[0069] Synthesis of methanone (surface modified compound (II)): 3-aminopropyltrimethoxysilane (APS) (0.72 g, 4 mmol), 3-(bromomethyl)benzophenone (1.1 g, 4 mmol) and potassium carbonate (0.72 g, 5.2 mmol) were dissolved in 6 ml of DMF, protected from light, and reacted at room temperature for 3 hours to precipitate a white solid. The solid was filtered, dried with water, rinsed with methanol, and dried to obtain the surface modified compound (II).
[0070] 2) Pretreatment of the quartz plate: rinse the quartz plate with 0.1 mol / L HCl solution for 30 min, then rinse with deionized water for 10 min, rinse the quartz plate with 0.1 mol / L NaOH solution for 2 h, then rinse with methanol for 10 min, and finally blow dry with nitrogen.
[0071] 3) Connecting the surface modified compound (II) to the treated quartz plate: prepare a mixed solution of the surface modified compound (II) and DMF (take 10 mg of the surface modified compound (II) and dissolve it in 30 mL of DMF), then add the solution into a square culture dish, immerse the quartz plate in the square culture dish and completely cover it with the mixed solution, then place the square culture dish in a 37° oven to react for 12-16 hours to complete the connection, then rinse with methanol for 10 minutes, and finally blow dry with nitrogen for use.
[0072] 4) Protein solidification treatment: Use a pipette to take 3 μL of protein sample (HRP protein - concentration 10 ng / μL) and add it to five different positions on the surface of the quartz plate treated in step 3), then irradiate at a wavelength of 350 mm for more than 30 minutes. After irradiation, use PBST to rinse the surface of the quartz plate, and finally spread the ultra-sensitive ECL luminescent liquid on the surface of the quartz plate. Use the 6000pro II luminescent camera produced by Guangzhou Boluteng Biotechnology Co., Ltd. to record the protein fixation effect.
[0073] Comparative Example 2: Similarly, a pipette was used to draw 3uL of protein sample (HRP protein - concentration 10ng / μL) to five different positions on the surface of the quartz plate treated in step 3). The difference from the above is that Comparative Example 2 was not irradiated at a wavelength of 350mm, but was only placed in a dark environment (the placement time was consistent with the irradiation time in step 4)), and then PBST was used to rinse the surface of the quartz plate, and finally the ultra-sensitive ECL luminescent liquid was spread all over the surface of the quartz plate, and 6000pro II was used to take photos and record the luminescence.
[0074] The results of the photo recording are shown in Table 2 and Figure 2 As shown, it can be seen from the experimental result diagram that there is an obvious difference in the results of signal detection after adding ECL luminescent liquid to the two modified quartz plates with and without irradiation after adding the protein sample. The average maximum signal of the five points of Example 2 treated with irradiation is about 21000 cts, while the average maximum signal of the five points of Control Example 2 not treated with irradiation is about 2500 cts. Therefore, the signal of Example 2 treated with irradiation is obviously greater than the signal of Control Example 2.
[0075] Table 2 Signal values of Example 2 and Comparative Example 2
[0076]
[0077] Example 3: Testing of modified PDMS
[0078] 1) Synthesis of pent-4-en-1-yl 2-(3-benzoy l pheny l)propanoate (surface-modified compound (III)): Ketoprofen (2.54 g, 10 mmol) and 4-penten-1-ol (1.44 ml, 12 mmol) were dissolved in 30 ml DMF, DMAP (0.12 g, 1 mmol) was added and stirred for 5 minutes, then EDC 1 (4.79 g, 25 mmol) was added and reacted at room temperature for 15 hours, extracted with water and ethyl acetate, spin-dried, and purified by silica gel column to obtain surface-modified compound (III).
[0079] 2) The PDMS-Si-H membrane is a PDMS sheet whose surface is hydrogenated after being treated with dilute hydrochloric acid, including but not limited to those purchased from Hangzhou Weisi Co., Ltd.
[0080] 3) Place the PDMS-Si-H membrane described in step 2) into a 25 ml isopropanol dry solution containing 2 grams of surface modification compound (III). Use a quartz dropper to draw 0.5 ml of Karstedts Pt catalyst, add it to the reaction system after activation at 80°C, mix well, and react at 35°C for 12-16 hours. After the reaction is completed, wash it with acetone and distilled water several times, vacuum dry it at 50°C for 4 hours, and take it out for use. (The membrane changes from transparent to milky white and opaque)
[0081] (4) 3 μl of protein (HRP protein - concentration 10 ng / μL) was respectively aspirated and dropped on five different locations on the dried membrane, and then irradiated at 350 mm for 30 min. Finally, the membrane was washed with PBST and water for 15 min, and then ECL luminescent solution was added for signal detection.
[0082] Comparative Example 3: Similarly, a pipette was used to draw 3uL of protein sample (HRP protein - concentration 10ng / μL) to five different positions on the membrane dried in step 3). The difference from the above is that Comparative Example 3 was not irradiated at a wavelength of 350mm, but was only placed in a dark environment (the placement time was consistent with the irradiation time in step 4)). Finally, the membrane was washed with PBST and water for 15 minutes, and then ECL luminescent liquid was added for signal detection.
[0083] The results of the photo recording are shown in Table 3 and Figure 3 As shown, it can be seen from the experimental result diagram that there is an obvious difference in the results of signal detection after adding ECL luminescent liquid to the two membranes with and without irradiation after adding the protein sample. The average maximum signal of the five points of Example 3 after irradiation is about 24000 cts, while the average maximum signal of the five points of Control Example 3 without irradiation is about 4000 cts. Therefore, the signal of Example 3 after irradiation is obviously greater than the signal of Control Example 3, which indicates that the modification and grafting of the board is successful.
[0084] Table 3 Signal values of Example 3 and Comparative Example 3
[0085]
[0086] Example 4: Testing of modified PMMA:
[0087] 1) Synthesis of 2-(3-benzoyl phenyl)-N-(3-(triethoxys ilyl)propy l)propanamide (surface-modified compound (IV)): Ketoprofen (2.54 g, 10 mmol) and 3-aminopropyltrimethoxysilane (2.8 ml, 12 mmol) were dissolved in 30 ml DMF, DMAP (0.12 g, 1 mmol) was added and stirred for 5 minutes, then EDC 1 (4.79 g, 25 mmol) was added and reacted at room temperature for 15 hours, extracted with water and ethyl acetate, dried by spin drying, and purified by silica gel column to obtain surface-modified compound (IV) as a transparent oily product.
[0088] 2) Use a plasma cleaning machine to clean the PMMA plate (conditions: time 120s, power 210W, gas is oxygen), and immediately soak it in 30ml methanol alkaline solution of the surface modification compound (IV) (30mg of the surface modification compound (IV) is dissolved in 30ml methanol and then 3ml of 1M NaOH aqueous solution is added), and the grafting reaction is carried out at 35°C overnight in the dark, and finally it is cleaned with methanol for 15min and set aside.
[0089] 3) After the plate surface was fully dried with a negative ion hair dryer, 3uL of protein sample (HRP protein - concentration 10ng / μL) was added to five different locations on the surface, and then irradiated at 350mm for more than half an hour. Finally, the plate was cleaned with PBST and 20% ammonium chloride solution and then ECL luminescence detection was performed (exposure time: 2s, binging: 4*4).
[0090] Comparative Example 4: Similarly, 3uL of protein sample ((HRP protein - concentration 10ng / μL)) was taken with a pipette and added dropwise to five different positions on the surface of the PMMA plate that had been treated in step 2). The difference from the above was that the control group was not irradiated at a wavelength of 350mm, but was only placed in a dark environment (the placement time was consistent with the irradiation time in step 3)), and then the plate was finally cleaned with PBST and 20% ammonium chloride solution, and then luminescence detection was performed by ECL, and luminescence photography was recorded using 6000pro II.
[0091] The experimental data are shown in Table 4 and Figure 4 As shown, it can be seen from the experimental results that there is an obvious difference in the results of signal detection after adding ECL luminescent liquid to the two PMMA plates with and without irradiation after adding the protein sample. The average maximum signal of the five points of Example 4 treated with irradiation is about 18000 cts, while the average maximum signal of the five points of Control Example 4 not treated with irradiation is about 1500 cts. Therefore, the signal of Example 4 treated with irradiation is obviously greater than the signal of Control Example 4.
[0092] Table 4 Signal values of Example 4 and Comparative Example 4
[0093]
[0094] The above embodiments are preferred implementation modes of the present invention, but the implementation modes of the present invention are not limited to the above embodiments. Any other changes, modifications, substitutions, combinations, and simplifications that do not deviate from the spirit and principles of the present invention should be equivalent replacement methods and are included in the protection scope of the present invention.
Claims
1. A surface-modified compound, characterized in that: Its chemical structure is shown in formula (I): Wherein R1 is selected from R2 is selected from H2 or CH3.
2. The surface modification compound according to claim 1, characterized in that The chemical structure is shown in formula (II), formula (III) or formula (IV):
3. A modified quartz plate, characterized in that: The surface modification compound is grafted onto a pretreated quartz plate, wherein the chemical structure of the surface modification compound is the formula (II) as described in claim 2.
4. The modified quartz plate according to claim 3, characterized in that: The pretreatment is to rinse the quartz plate with 0.1 mol / L HCl solution for 30 minutes, then rinse with deionized water for 10 minutes, rinse the quartz plate with 0.1 mol / L NaOH solution for 2 hours, then rinse with methanol for 10 minutes, and finally blow dry with nitrogen.
5. A method for preparing the modified quartz plate according to claim 3, characterized in that: The preparation steps are as follows: 1) Pre-treat the quartz plate; 2) Grafting 3-aminopropyltrimethoxysilane onto the quartz plate: prepare a mixed solution of 3-aminopropyltrimethoxysilane and methanol, add the solution into a square culture dish, immerse the quartz plate in the mixed solution, place the square culture dish in an oven for reaction, rinse with methanol, and finally dry with nitrogen for later use; 3) Connecting 3-(bromomethyl)benzophenone to 3-aminopropyltrimethoxysilane: using DMF to dissolve 3-(bromomethyl)benzophenone and potassium carbonate powder, after light protection and ultrasound, a mixed solution is formed; then the quartz plate treated in step 2) is immersed in the mixed solution, reacted at room temperature, and after the connection is completed, rinsed with DMF, then rinsed with PBST, and finally dried with nitrogen to obtain a modified quartz plate.
6. A method for preparing the modified quartz plate as claimed in claim 3, characterized in that: The preparation steps are as follows: 1) Synthesis of surface modified compound: 3-aminopropyltrimethoxysilane, 3-(bromomethyl)benzophenone and potassium carbonate were dissolved in DMF, protected from light, reacted at room temperature, a white solid was precipitated, filtered, dried with water, rinsed with methanol, and dried to obtain a surface modified compound; 2) Pre-treating the quartz plate; 3) Connecting the surface modification compound to the treated quartz plate: prepare a mixed solution of the surface modification compound and DMF, add the solution into a square culture dish, and then immerse the quartz plate in the mixed solution until the quartz plate is completely covered by the mixed solution. Then place the square culture dish in an oven for reaction, rinse after the connection is completed, and finally blow dry with nitrogen to obtain a modified quartz plate.
7. A modified PDMS plate, characterized in that: The surface modification compound is grafted onto a hydrosilane treated PDMS plate, wherein the chemical structure of the surface modification compound is as shown in the formula (III) of claim 2.
8. A method for preparing the modified PDMS plate as claimed in claim 7, characterized in that: The preparation steps are as follows: 1) Synthesis of surface modified compound: ketoprofen and 4-penten-1-ol were dissolved in DMF, DMAP was added and stirred, EDCl was added, reaction was performed at room temperature, extraction was performed by spin drying, and purification was performed to obtain a surface modified compound; 2) placing the PDMS-Si-H membrane into a drying solution of isopropanol containing a surface modification compound; Use a quartz dropper to draw up the Karstedts Pt catalyst, add it into the reaction system after activation, mix it evenly and then react; After the reaction is completed, the modified PDMS plate is obtained by washing several times and vacuum drying.
9. A modified PMMA plate, characterized in that: The surface modification compound is grafted onto a PMMA plate after plasma cleaning, wherein the chemical structure of the surface modification compound is as shown in formula (IV) as claimed in claim 2.
10. A method for preparing the modified PMMA plate as claimed in claim 9, characterized in that: The preparation steps are as follows: 1) Synthesis of surface-modified compound: ketoprofen and 3-aminopropyltrimethoxysilane were dissolved in DMF, DMAP was added and stirred, EDCl was added, reacted at room temperature, extracted, spin-dried, and purified to obtain a surface-modified compound in the form of a transparent oil; 2) Clean the PMMA plate with a plasma cleaner, and immediately soak it in a methanol alkaline solution of the surface modification compound obtained in step 1) after cleaning, and allow the grafting reaction to proceed overnight in the dark, and finally clean it with methanol to obtain the modified PMMA plate.
Citation Information
Patent Citations
Difunctional polymer and modification method
CN115677922A
Coating and preparation method thereof, coating and preparation method of biological material containing coating
CN117417676A
Method for catalyzing hydrogenation of carbon-carbon double bonds by using electrically driven platinum catalyst and application of method
CN117779067A
Electrically conductive polymers capable of being covalently grafted on by light, method for obtaining same and uses as supports in probes for specific identification in electronic biosensors
US7034164B1