Biomass-based resin as well as preparation method and application thereof

A method for preparing biomass-based resins through thermal polymerization and reaction with bio-based carboxylic acid addresses high cost and environmental issues, producing a tear-resistant resin suitable for automotive and packaging applications.

CN119081007AInactive Publication Date: 2024-12-06HENGHE MATERIALS & SCI TECH CO LTD
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202411571459.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-11-06
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

Traditional methods for preparing biomass-based tear-resistant resins face issues such as high cost, complex processes, environmental pollution, high molecular weight, poor tear resistance, and harsh reaction conditions, which limit their application in fields like automobile tires and packaging materials.

Method used

A method involving thermal free radical polymerization of cyclopentadiene and norbornene monomers, followed by reaction with a bio-based carboxylic acid using a modified phosphotungstic acid catalyst, to produce a biomass-based resin with improved tear resistance and reduced molecular weight.

Benefits of technology

The method results in a tear-resistant biomass-based resin with enhanced compatibility and viscosity, suitable for automotive parts and packaging materials, under milder conditions and with reduced environmental impact.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081007A_ABST
    Figure CN119081007A_ABST
Patent Text Reader

Abstract

The invention discloses biomass-based resin as well as a preparation method and application thereof, and belongs to the technical field of bio-based materials. The preparation method comprises the following steps: carrying out a thermal free radical polymerization reaction on cyclopentadiene and derivatives thereof and norbornene monomers in the presence of a first solvent, adding a straight-chain ether compound for continuous reaction, separating out a cycloolefin copolymer, and carrying out a reaction on the cycloolefin copolymer and bio-based carboxylic acid in the presence of a second solvent and a catalyst. The method is simple in process, easy to operate and mild in condition, and the biomass-based resin with excellent physical and chemical properties and tackifying performance can be obtained; the biomass-based resin can effectively increase the viscosity of a sizing material, has good compatibility with rubber, and can improve the tear resistance and chunking and chipping resistance of the sizing material. Besides, the biomass-based resin has good dynamic performance and higher modulus, is helpful for improving the processability of rubber materials, and can be applied to the fields of automobile spare parts, packaging materials or electronic equipment and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of bio-based materials, and in particular to a biomass-based resin and a preparation method and application thereof. Background Art

[0002] In the current context of increasing global environmental awareness, biomass-based materials have received extensive attention and research due to their renewable and degradable properties. Among them, biomass-based tear-resistant resins, as an important biomass-based material, are widely used in various fields, such as automobile tires, packaging materials, electronic equipment, etc. However, the traditional preparation methods of biomass-based tear-resistant resins often have problems such as high cost, complex process, and environmental pollution.

[0003] Safety and durability are the two most important properties of automobile tires. It is difficult to take into account both wet skid resistance, wear resistance and rolling resistance, which are used to measure the above properties, and they will affect each other. With the rapid development of domestic high-end new energy vehicles, low-aspect ratio, large inner diameter, high-speed and high-pressure tires with good sensitivity and acceleration performance have become the mainstream development trend, thus placing higher demands on the tear resistance of tire rubber.

[0004] At present, some technologies use rosin resin to modify rubber materials to improve the tear resistance of tire rubber. The main component of rosin resin is rosin resin acid, which is a carboxylic acid with a tricyclic phenanthrene skeleton and two double bonds. It has a high softening point, but its active group has a large steric hindrance in chemical reaction. Therefore, modification with rosin resin often requires higher temperature and harsher reaction conditions.

[0005] In addition, as far as the preparation method of biomass-based resin itself is concerned, it still has the following problems: First, a large amount of organic solvents are required in the preparation process, which is not conducive to reducing costs and protecting the environment; second, the molecular weight of the biomass-based resin prepared by the existing method is relatively large, which limits its application; third, the tear resistance of the biomass-based resin prepared by the existing method is still poor; fourth, the preparation process conditions of biomass-based resin are relatively harsh, the cost is high, and the scope of application is limited.

[0006] In view of this, the present invention is proposed. Summary of the invention

[0007] The object of the present invention is to provide a biomass-based resin and a preparation method and application thereof, so as to solve or improve at least one of the above-mentioned technical problems.

[0008] The present invention can be implemented like this: In a first aspect, the present invention provides a method for preparing a biomass-based resin, comprising the following steps: Conducting a thermal free radical polymerization reaction of cyclopentadiene and its derivatives with norbornene monomers in the presence of a first solvent, and then adding a linear ether compound to continue the reaction to obtain a first polymerization solution containing a cycloolefin copolymer; The cyclic olefin copolymer in the first polymerization solution is separated, and the separated cyclic olefin copolymer is reacted with a bio-based carboxylic acid in the presence of a second solvent and a catalyst to obtain a biomass-based resin.

[0009] In an optional embodiment, preparing the first polymer solution includes at least one of the following features: Feature 1: The temperature of the thermal free radical polymerization reaction is 100°C~250°C, the pressure is 0.15MPa~2.0MPa, and the time is 0.5h~5.0h; Feature 2: The mass ratio of cyclopentadiene and its derivatives to norbornene monomers is 1:0.1 to 1:2.0; Feature 3: The first solvent accounts for 15% to 50% of the total material mass, and the total material is the sum of cyclopentadiene and its derivatives, norbornene monomers and linear ether compounds; Feature 4: After adding the linear ether compound, the temperature for continuing the reaction is 100°C to 250°C, the pressure is 0.15MPa to 2.0MPa, and the time is 1.0h to 10h; Feature 5: The amount of the linear ether compound added is 0.1% to 5% of the total material mass, and the total material is the sum of cyclopentadiene and its derivatives, norbornene monomers and linear ether compounds; Feature 6: Cyclopentadiene and its derivatives include at least one of cyclopentadiene, methylcyclopentadiene, dimethylcyclopentadiene, dicyclopentadiene, methylcyclopentadiene dimer and cyclopentadiene-methylcyclopentadiene dimer; Feature 7: The norbornene monomer includes at least one of norbornene, 2,5-norbornadiene, 5-vinyl-2-norbornene, 5-ethylidene-2-norbornene and 2-allyl-5-norbornene; Feature 8: The first solvent includes decahydronaphthalene; Feature 9: The straight-chain ether compound includes a divinyl ether monomer.

[0010] In an optional embodiment, the linear ether compound includes at least one of divinyl ether, diethylene glycol divinyl ether, 1,4-butanediol divinyl ether, 1,6-hexanediol divinyl ether and 1,4-cyclohexanedimethanol divinyl ether.

[0011] In an alternative embodiment, separating the cyclic olefin copolymer in the first polymer solution comprises at least one of the following features: Feature 10: Separating the cycloolefin copolymer in the first polymerization solution by flash evaporation; wherein the flash evaporation pressure is 20 kPa to 80 kPa, and the flash evaporation temperature is 180° C. to 250° C.; Feature 11: The Gardner color number of the separated cycloolefin copolymer is ≤4.0#, the melt viscosity at 40°C is ≤3000 mPa·s, and the Z-average molecular weight is ≤1500.

[0012] In an alternative embodiment, the reaction of the cyclic olefin copolymer with the bio-based carboxylic acid includes at least one of the following features: Feature 12: The reaction temperature of the cyclic olefin copolymer and the bio-based carboxylic acid is 50°C to 120°C, the reaction pressure is 0.1MPa to 1.0MPa, and the reaction time is 0.25h to 2.0h; Feature 13: The mass ratios of the cyclic olefin copolymer, the bio-based carboxylic acid, and the second solvent are 1:(0.7-1.5):(0.75-10) respectively; Feature 14: The bio-based carboxylic acid includes at least one of 3-hydroxypropionic acid, 2,5-furandicarboxylic acid, abietic acid, dehydroabietic acid, dehydroabietic acid, 2,2-dimethylsuccinic anhydride, allylsuccinic anhydride, butylsuccinic anhydride, 2-octenylsuccinic anhydride, ricinoleic acid, dehydrated ricinoleic acid, itaconic acid and hexylitaconic acid; Feature 15: The second solvent includes benzene, cyclohexane and its derivatives; Feature 16: The catalyst includes a phosphotungstic acid catalyst; Feature 17: The reaction of the cyclic olefin copolymer and the bio-based carboxylic acid is carried out in a fixed bed reactor.

[0013] In an alternative embodiment, the second solvent comprises methylcyclohexane and benzene.

[0014] In an optional embodiment, the mass ratio of methylcyclohexane to benzene is 1:0.5 to 1:1.0.

[0015] In an alternative embodiment, the catalyst is a modified phosphotungstic acid catalyst.

[0016] In an optional embodiment, the modified phosphotungstic acid catalyst is obtained by loading modified tungsten phosphate on a carrier, wherein the molecular formula of the modified tungsten phosphate is Cs (0.5~2.5) H (0.5~2.5) PW 12 O 40 The mass ratio of the modified tungsten phosphate to the carrier is 0.5:99.5 to 50:50.

[0017] In an optional embodiment, the carrier includes at least one of H-ZMS-5, SBA-15, USY molecular sieve and hydroxyl-containing mesoporous silica.

[0018] In an optional embodiment, the separated cyclic olefin copolymer is firstly freed from impurities in a packed tower, and then reacted with a bio-based carboxylic acid and a second solvent in the presence of a catalyst; The filler used in the packed tower includes at least one of α-alumina and diatomaceous earth.

[0019] In an alternative embodiment, the packing in the packed tower contains both α-alumina and diatomaceous earth.

[0020] In an optional embodiment, the volume ratio of α-alumina and diatomaceous earth contained in the packed tower is 1:0.2 to 1:1.5.

[0021] In an optional embodiment, the method for preparing the biomass-based resin further comprises: post-treating the second polymer solution obtained by reacting the cyclic olefin copolymer with the bio-based carboxylic acid; The post-treatment includes: removing the unreacted monomers and the remaining solvent and oligomers in the second polymerization liquid; wherein, the unreacted monomers are eluted with organic alcohol, and the remaining solvent and oligomers are removed by distillation.

[0022] In an alternative embodiment, the organic alcohol comprises at least one of methanol, ethanol and propanol.

[0023] In an optional embodiment, the mass ratio of the second polymerization liquid to the organic alcohol is 1:0.05 to 1:0.50.

[0024] In an optional embodiment, the distillation is carried out under the conditions of 20 kPa to 50 kPa and 180° C. to 280° C.

[0025] In an optional embodiment, the method for preparing the biomass-based resin further comprises: recovering the light component remaining after the cycloolefin copolymer is separated from the first polymerization liquid to obtain the first solvent in the light component; Wherein, the recovery of light components includes at least one of the following characteristics: Feature 18: Use microporous membrane to separate light components; Feature 19: Separation of light components is carried out under conditions of 15°C ~ 35°C and 0.1MPa ~ 0.3MPa.

[0026] In an alternative embodiment, the microporous membrane comprises a polyvinylidene fluoride filter membrane.

[0027] In an alternative embodiment, the recovered first solvent is returned to the thermal free radical polymerization process.

[0028] In a second aspect, the present invention provides a biomass-based resin, which is prepared by the preparation method of any one of the aforementioned embodiments.

[0029] In an optional embodiment, the biomass-based resin has at least one of the following characteristics: Feature 20: The softening point of the biomass-based resin is 80°C to 140°C, preferably 95°C to 120°C; Feature 21: The Gardner color number of the biomass-based resin is ≤8#, preferably ≤6.5#; Feature 22: The acid value of the biomass-based resin is 50 mgKOH / g to 500 mgKOH / g, preferably 50 mgKOH / g to 150 mgKOH / g; Feature 23: The iodine value of the biomass-based resin is 10gI2 / 100g~300gI2 / 100g, preferably 70gI2 / 100g~180gI2 / 100g.

[0030] In a third aspect, the present invention provides a composite material, wherein the raw materials for preparing the composite material include a rubber material and the biomass-based resin of the aforementioned embodiment; In an optional embodiment, the rubber material includes at least one of natural rubber, synthetic rubber and elastomer.

[0031] In an optional embodiment, the rubber material includes at least one of butadiene rubber, styrene butadiene rubber, natural rubber and SBC elastomer.

[0032] In a fourth aspect, the present invention provides the use of the composite material according to the aforementioned embodiment in automotive parts, packaging materials or electronic devices; In an optional embodiment, the automobile spare parts include automobile tires or automobile interior decoration.

[0033] The beneficial effects of the present invention include: The present invention first generates cyclic molecules by Diels-Alder reaction of cyclopentadiene and its derivatives with norbornene monomers in the free radical polymerization of cycloolefin copolymers, and then reduces the generation of macromolecular gel substances in the polymerization reaction by adding a proper amount of linear ether compounds as molecular weight regulators during the reaction, thereby obtaining a liquid cycloolefin copolymer with low viscosity and low Z-average molecular weight. By using the cycloolefin copolymer as a reaction intermediate and reacting it with a bio-based carboxylic acid in the presence of a second solvent and a catalyst, a tear-resistant biomass-based resin can be obtained under milder reaction conditions and a simpler production process.

[0034] The tear-resistant biomass-based resin can improve the tear resistance and chipping resistance of the rubber, effectively increase the viscosity of the rubber and have good compatibility with rubber. In addition, the tear-resistant biomass-based resin also has good dynamic performance and high modulus, which helps to improve the cutting resistance of the tread rubber and improve the processing performance of the rubber rubber. The tear-resistant biomass-based resin can be used in automotive parts (including rubber tires, automotive interiors, automotive anti-damping parts, etc.), packaging materials or electronic equipment and other fields. BRIEF DESCRIPTION OF THE DRAWINGS

[0035] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.

[0036] Figure 1 This is a process flow chart of the method for preparing biomass-based resin provided in Example 1 of the present invention.

[0037] Icons: R101-high pressure reactor; T101-flash tower; T102-packed tower; R102-fixed bed reactor; V101-alcohol washing kettle; T103-distillation tower. DETAILED DESCRIPTION

[0038] In order to make the purpose, technical scheme and advantages of the embodiments of the present invention clearer, the technical scheme in the embodiments of the present invention will be described clearly and completely below. If the specific conditions are not specified in the embodiments, they are carried out according to conventional conditions or conditions recommended by the manufacturer. If the manufacturer of the reagents or instruments used is not specified, they are all conventional products that can be purchased commercially.

[0039] The biomass-based resin provided by the present invention and its preparation method and application are described in detail below.

[0040] The present invention provides a method for preparing a biomass-based resin, comprising the following steps: Conducting a thermal free radical polymerization reaction of cyclopentadiene and its derivatives with norbornene monomers in the presence of a first solvent, and then adding a linear ether compound to continue the reaction to obtain a first polymerization solution containing a cycloolefin copolymer; The cyclic olefin copolymer in the first polymerization solution is separated, and the separated cyclic olefin copolymer is reacted with a bio-based carboxylic acid in the presence of a second solvent and a catalyst to obtain a biomass-based resin.

[0041] In some optional embodiments, the temperature of the thermal free radical polymerization reaction can be 100°C to 250°C, such as 100°C, 120°C, 150°C, 180°C, 200°C, 220°C or 250°C, etc., or other values ​​within the range of 100°C to 250°C.

[0042] If the temperature of the thermal free radical polymerization reaction is lower than 100°C, it is not conducive to the growth of the polymer reaction chain and the reaction is slow; if the temperature of the thermal free radical polymerization reaction is higher than 250°C, the free radical polymerization activity of cyclopentadiene and its derivatives is too high, and a large amount of insoluble high molecular weight polymers, also known as explosive polymer "slag", are easily generated, affecting the reaction yield.

[0043] The pressure of the thermal free radical polymerization reaction can be 0.15 MPa to 2.0 MPa, such as 0.15 MPa, 0.5 MPa, 0.8 MPa, 1.0 MPa, 1.2 MPa, 1.5 MPa, 1.8 MPa or 2.0 MPa, or other values ​​within the range of 0.15 MPa to 2.0 MPa.

[0044] The time of the thermal free radical polymerization reaction can be 0.5h~5.0h, such as 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h or 5h, or other values ​​within the range of 0.5h~5.0h.

[0045] If the thermal free radical polymerization reaction time is shorter than 0.5 h, it is not conducive to obtaining the desired polymer with a suitable relative molecular mass; if the thermal free radical polymerization reaction time is longer than 5.0 h, it is easy to generate a large amount of high molecular weight polymer and affect the molecular structure of the cycloolefin polymer.

[0046] In some optional embodiments, the mass ratio of cyclopentadiene and its derivatives to norbornene monomers can be 1:0.1 to 1:2.0, such as 1:0.1, 1:0.2, 1:0.5, 1:0.8, 1:10, 1:1.2, 1:1.5, 1:1.8 or 1:2.0, or other values ​​within the range of 1:0.1 to 1:2.0.

[0047] Wherein, cyclopentadiene and its derivatives may illustratively but not limitatively include at least one of cyclopentadiene, methylcyclopentadiene, dimethylcyclopentadiene, dicyclopentadiene, methylcyclopentadiene dimer and cyclopentadiene-methylcyclopentadiene dimer.

[0048] The norbornene-based monomer may illustratively but not limitatively include at least one of norbornene, 2,5-norbornadiene, 5-vinyl-2-norbornene, 5-ethylidene-2-norbornene, and 2-allyl-5-norbornene.

[0049] In some optional embodiments, the first solvent may be 15% to 50% of the total mass of the material, such as 15%, 20%, 25%, 30%, 35%, 40%, 45% or 50%, etc., or other values ​​within the range of 15% to 50%. The above-mentioned "total material" is the sum of cyclopentadiene and its derivatives, norbornene monomers and linear ether compounds, the same below.

[0050] The first solvent may include decahydronaphthalene by way of example but not limitation. In some typical embodiments, the first solvent is decahydronaphthalene. By using decahydronaphthalene as the first solvent, cyclopentadiene and its derivatives and norbornene monomers can be effectively dissolved on the one hand, and the reaction can be controlled not to be too violent on the other hand.

[0051] In some optional embodiments, the temperature for continuing the reaction after adding the linear ether compound can be 100°C~250°C, such as 100°C, 120°C, 150°C, 180°C, 200°C, 220°C or 250°C, etc., or other values ​​within the range of 100°C~250°C.

[0052] The pressure for continuing the reaction after adding the linear ether compound can be 0.15MPa~2.0MPa, such as 0.15MPa, 0.5MPa, 0.8MPa, 1.0MPa, 1.2MPa, 1.5MPa, 1.8MPa or 2.0MPa, etc., or other values ​​within the range of 0.15MPa~2.0MPa.

[0053] The reaction time after adding the linear ether compound can be 1.0h~10h, such as 0.5h, 1h, 1.5h, 2h, 2.5h, 3h, 3.5h, 4h, 4.5h, 5h, 5.5h, 6h, 6.5h, 7h, 7.5h, 8h, 8.5h, 9h, 9.5h or 10h, etc., or other values ​​within the range of 0.5h~10.0h.

[0054] The addition amount of the linear ether compound can be 0.1% to 5% of the total material mass, such as 0.1%, 0.2%, 0.5%, 1%, 1.5%, 2%, 2.5%, 3%, 3.5%, 4%, 4.5% or 5%, etc., or other values ​​within the range of 0.1% to 5%.

[0055] Among them, the straight-chain ether compound includes divinyl ether monomers, and the divinyl monomers can illustratively but not limitatively include at least one of divinyl ether, diethylene glycol divinyl ether, 1,4-butanediol divinyl ether, 1,6-hexanediol divinyl ether and 1,4-cyclohexanedimethanol divinyl ether.

[0056] As mentioned above, by free radical polymerization of cyclopentadiene and its derivatives with norbornene monomers at high temperature, and adding linear ethers to participate in the copolymerization reaction at the right time, a low molecular weight, performance-adjustable cycloolefin copolymer can be obtained. In other words, in the free radical polymerization of cycloolefin copolymers, cyclopentadiene and norbornene monomers are first generated by Diels-Alder reaction to form cyclic molecules, and then by adding linear ether compounds as molecular weight regulators in the reaction process, the generation of macromolecular gel substances in the polymerization reaction is reduced, thereby obtaining a liquid cycloolefin copolymer with low viscosity and low Z-average molecular weight. In addition, it should be emphasized that if linear ether compounds are not added to S1, the catalytic copolymerization efficiency of the prepared cycloolefin copolymer with bio-based carboxylic acid will be low, and the overall acid value and iodine value will be significantly reduced.

[0057] In some optional embodiments, the cycloolefin copolymer in the first polymerization solution can be separated by flash evaporation. Exemplarily, the pressure of the flash evaporation can be 20kPa~80kPa, such as 20kPa, 25kPa, 30kPa, 35kPa, 40kPa, 45kPa, 50kPa, 55kPa, 60kPa, 65kPa, 70kPa, 75kPa or 80kPa, etc., or other values ​​within the range of 20kPa~80kPa. The temperature of the flash evaporation can be 180℃~250℃, such as 180℃, 190℃, 200℃, 210℃, 220℃, 230℃, 240℃ or 250℃, etc., or other values ​​within the range of 180℃~250℃.

[0058] Flash evaporation under the above conditions can remove the first solvent and unreacted monomers, and effectively separate the light component from the cycloolefin copolymer.

[0059] In some optional embodiments, the Gardner color number of the separated cyclic olefin copolymer is ≤4.0#, such as 1.5#~1.8#, such as 1.5#, 1.6# or 1.8#.

[0060] In some optional embodiments, the melt viscosity of the separated cycloolefin copolymer at 40° C. is ≤3000 mPa·s, such as 1233 mPa·s to 1720 mPa·s, such as 1233 mPa·s, 1374 mPa·s, 1555 mPa·s or 1720 mPa·s.

[0061] In some optional embodiments, the Z average molecular weight (Mz) of the separated cycloolefin copolymer is ≤1500, such as 875-1360, such as 875, 986, 1088 or 1360.

[0062] In some optional embodiments, the light components remaining after the cycloolefin copolymer is separated from the first polymerization liquid can be recovered to obtain the first solvent in the light components. The recovered first solvent can be returned to the thermal free radical polymerization process.

[0063] For example, a microporous membrane may be used to separate the light component. The microporous membrane may be, for example, a polyvinylidene fluoride filter membrane. The separation of the light component may be performed under conditions of 15°C to 35°C (e.g., 15°C, 20°C, 25°C, 30°C, or 35°C, etc.) and 0.1MPa to 0.3MPa (e.g., 0.1MPa, 0.15MPa, 0.2MPa, 0.25MPa, or 0.3MPa, etc.).

[0064] In some preferred embodiments, the separated cycloolefin copolymer can be firstly freed from impurities in a packed tower, and then reacted with the bio-based carboxylic acid and the second solvent in the presence of a catalyst. The reaction process can be carried out in a fixed bed reactor.

[0065] For example, the filler used in the packed tower includes at least one of α-alumina and diatomaceous earth. Preferably, the filler in the packed tower contains both α-alumina and diatomaceous earth, and accordingly, the volume ratio of α-alumina and diatomaceous earth contained in the packed tower can be 1:0.2 to 1:1.5, such as 1:0.2, 1:0.5, 1:0.8, 1:1, 1:1.2 or 1:1.5, etc., and can also be other values ​​within the range of 1:0.2 to 1:1.5.

[0066] In some optional embodiments, the reaction temperature of the cyclic olefin copolymer and the bio-based carboxylic acid can be 50°C to 120°C, such as 50°C, 60°C, 70°C, 80°C, 90°C, 100°C, 110°C or 120°C, etc., or other values ​​within the range of 50°C to 120°C.

[0067] The reaction pressure of the cyclic olefin copolymer and the bio-based carboxylic acid can be 0.1 MPa to 1.0 MPa, such as 0.1 MPa, 0.2 MPa, 0.3 MPa, 0.4 MPa, 0.5 MPa, 0.6 MPa, 0.7 MPa, 0.8 MPa, 0.9 MPa or 1.0 MPa, etc., or other values ​​within the range of 0.1 MPa to 1.0 MPa.

[0068] The reaction time of the cyclic olefin copolymer and the bio-based carboxylic acid can be 0.25 h to 2.0 h, such as 0.25 h, 0.5 h, 1 h, 1.5 h or 2 h, or other values ​​within the range of 0.25 h to 2.0 h.

[0069] The mass ratio of the cycloolefin copolymer to the bio-based carboxylic acid and the second solvent can be 1:(0.7-1.5):(0.75-10), such as 1:0.7:0.75, 1:0.7:1, 1:0.7:2, 1:0.7:3, 1:0.7:4, 1:0.7:5, 1:0.7:6, 1:0.7:7, 1:0.7:8, 1:0.7:9, 1:0.7:10, 1:1:0.75, 1:1:1, 1:1:2, 1:1:3, 1:1:4, 1:1:5, 1:1:6, 1:1:7, 1:1:8, 1:1:9, 1:1:10, 1:1.5:0.75, 1:1.5:1, 1:1.5:2, 1:1.5:3, 1:1.5:4, 1:1.5:5, 1:1.5:6, 1:1.5:7, 1:1.5:8, 1:1.5:9, 1:1.5:10, etc., and can also be other values ​​within the range of 1:(0.7~1.5):(0.75~10).

[0070] Among them, the bio-based carboxylic acid can illustratively but not limitatively include at least one of 3-hydroxypropionic acid, 2,5-furandicarboxylic acid, abietic acid, dehydroabietic acid, dehydroabietic acid, 2,2-dimethylsuccinic anhydride, allylsuccinic anhydride, butylsuccinic anhydride, 2-octenylsuccinic anhydride, ricinoleic acid, dehydrated ricinoleic acid, itaconic acid and hexylitaconic acid.

[0071] The second solvent includes benzene and cyclohexane and its derivatives. In some typical embodiments, the second solvent may include methylcyclohexane and benzene, and the mass ratio of methylcyclohexane to benzene may be 1:0.5 to 1:1.0, such as 1:0.5, 1:0.6, 1:0.7, 1:0.8, 1:0.9 or 1:1, etc., or other values ​​within the range of 1:0.5 to 1:1.0.

[0072] The above-mentioned catalyst includes a phosphotungstic acid catalyst. In some preferred embodiments, the catalyst is a modified phosphotungstic acid catalyst, which is obtained by loading modified tungsten phosphate on a carrier, and the modifying element can exemplarily include cesium, and the carrier can exemplarily but not limitatively include at least one of H-ZMS-5, SBA-15, USY molecular sieve and hydroxyl-containing mesoporous silica.

[0073] As an example, the molecular formula of the modified tungsten phosphate can be Cs (0.5~2.5) H (0.5~2.5) PW 12 O 40 , such as Cs 0.5 H 2.5 PW 12 O 40 、Cs1H2PW 12 O 40 , Cs1.5 H 1.5 PW 12 O 40 、Cs2H1PW 12 O 40 or Cs 2.5 H 0.5 PW 12 O 40 wait.

[0074] The mass ratio of the modified tungsten phosphate to the carrier can be 0.5:99.5 to 50:50, such as 0.5:99.5, 1:99, 2:98, 5:95, 10:90, 15:85, 20:80, 25:75, 30:70, 35:65, 40:60, 45:55 or 50:50, or other values ​​within the range of 0.5:99.5 to 50:50.

[0075] In some embodiments, the preparation method of the modified phosphotungstic acid catalyst can refer to the following steps: Step (1): Add phosphotungstic acid, soluble cesium salt (such as cesium chloride, cesium nitrate and cesium sulfate, etc.) and water into a closed, stirred high-pressure reactor and stir thoroughly; Step (2): adding a pre-dried carrier into the reactor, and impregnating the carrier at 10°C to 60°C (e.g., 10°C, 20°C, 30°C, 40°C, 50°C, or 60°C, etc.), with a residence time of 0.5h to 5.0h (e.g., 0.5h, 1h, 2h, 3h, 4h, or 5h, etc.), so that a stable chemical bond is formed between the phosphotungstic acid and the carrier; Step (3): After the impregnation equilibrium is reached, the remaining liquid is removed, and the catalyst is dried in a vacuum oven at a temperature of 40°C to 120°C (such as 40°C, 60°C, 80°C, 100°C or 120°C, etc.) to obtain a loaded modified phosphotungstic acid catalyst.

[0076] As mentioned above, the present invention adopts a compound solvent as the second solvent, which can obtain a more suitable reaction polarity; the modified phosphotungstic acid catalyst used in the present invention has high catalytic activity and selectivity, can promote the chemical reaction, and improve the reaction rate and yield; secondly, the modified phosphotungstic acid catalyst is also environmentally friendly, does not produce harmful substances, and does not pollute the environment; finally, the modified phosphotungstic acid catalyst has a low cost and can be produced on a large scale.

[0077] By combining the compound solvent with the modified phosphotungstic acid catalyst, the catalytic polymerization activity of the bio-based carboxylic acid and cycloolefin copolymer can be effectively increased, the polymerization conversion rate of cycloolefin compounds and bio-based carboxylic acids can be effectively improved, the softening point and acid value of the product can be increased, the iodine value of the product can be reduced, and a biomass-based resin with excellent performance can be obtained.

[0078] As mentioned above, by using cycloolefin copolymer as a reaction intermediate and reacting with bio-based carboxylic acid with modified phosphotungstic acid as a catalyst, a tear-resistant biomass-based resin can be obtained under mild reaction conditions and a simple production process. The tear-resistant biomass-based resin can improve the tear resistance and anti-crushing properties of the rubber compound, effectively increase the viscosity of the rubber compound and have good compatibility with rubber. In addition, the tear-resistant biomass-based resin also has good dynamic properties and a high modulus, which helps to improve the cut resistance of the tread rubber and improve the processing properties of the rubber compound.

[0079] Furthermore, the second polymerization liquid obtained by reacting the cyclic olefin copolymer with the bio-based carboxylic acid is post-treated.

[0080] The post-treatment may include removing unreacted monomers and remaining solvents and oligomers in the second polymerization solution.

[0081] In some optional embodiments, an organic alcohol may be used to elute the unreacted monomer, and the organic alcohol may illustratively but not limitatively include at least one of methanol, ethanol and propanol. The mass ratio of the second polymer solution to the organic alcohol may be 1:0.05 to 1:0.50, such as 1:0.05, 1:0.10, 1:0.15, 1:0.20, 1:0.25, 1:0.30, 1:0.35, 1:0.40, 1:0.45 or 1:0.50, or other values ​​within the range of 1:0.05 to 1:0.50.

[0082] In some optional embodiments, the remaining solvent and oligomers can be removed by distillation. For example, the distillation can be carried out under the conditions of 20 kPa to 50 kPa (such as 20 kPa, 25 kPa, 30 kPa, 35 kPa, 40 kPa, 45 kPa or 50 kPa, etc.) and 180°C to 280°C (such as 180°C, 200°C, 220°C, 240°C, 260°C or 280°C, etc.).

[0083] Through post-processing, the impurity content can be reduced and the purity of biomass-based resin can be further improved.

[0084] Correspondingly, the present invention also provides a production system for preparing the above-mentioned biomass-based resin, the production system comprising a high-pressure reactor, a flash tower, a membrane separator, a packing tower, a reactor, an alcohol washing kettle and a distillation tower.

[0085] The high-pressure reactor is used for reacting cyclopentadiene and its derivatives, norbornene monomers and linear ether compounds; the bottom discharge port of the high-pressure reactor is connected to the feed port of the flash tower to separate the cycloolefin copolymer in the first polymerization liquid, the top of the flash tower obtains the light component, and the bottom of the tower obtains the cycloolefin copolymer; the inlet of the membrane separator is connected to the top of the flash tower, and the outlet of the membrane separator is connected to the high-pressure reactor, the first solvent in the light component can be recovered through the membrane separator, and the recovered first solvent can be returned to the high-pressure reactor for recycling; the bottom discharge port of the flash tower is connected to the bottom inlet of the packed tower, and the bottom of the tower is connected to the bottom of the packed tower. The packed tower removes impurities from the cycloolefin copolymer; the top outlet of the packed tower is connected to the bottom inlet of the reactor to allow the cycloolefin copolymer with impurities removed to react with the bio-based carboxylic acid introduced into the reactor; the reactor is a fixed bed reactor having a modified phosphotungstic acid catalyst inside; the top outlet of the reactor is connected to the top inlet of the alcohol washing kettle to elute unreacted monomers with organic alcohols in the alcohol washing kettle; the bottom outlet of the alcohol washing kettle is connected to the inlet of the distillation tower to remove the second solvent and the oligomers generated by the reaction, that is, the oligomers and the second solvent are obtained at the top of the distillation tower, and the biomass-based resin is obtained at the bottom of the distillation tower.

[0086] Correspondingly, the present invention also provides a biomass-based resin, which is prepared by the above preparation method.

[0087] In some optional embodiments, the softening point of the biomass-based resin is 80°C to 140°C, such as 80°C, 85°C, 90°C, 95°C, 100°C, 105°C, 110°C, 115°C, 120°C, 125°C, 130°C, 135°C or 140°C, etc., and may also be other values ​​within the range of 80°C to 140°C. In some more typical embodiments, the softening point of the biomass-based resin is 95°C to 120°C, and may further be 96.5°C to 120.0°C, such as 96.5°C, 99.4°C, 99.5°C, 101.2°C, 101.5°C, 102.8°C, 103.0°C, 104.8°C, 104.9°C, 105.2°C, 106.0°C or 120°C, etc.

[0088] In some optional embodiments, the Gardner color number of the biomass-based resin is ≤ 8#. In some typical embodiments, the Gardner color number of the biomass-based resin is ≤ 6.5#, and can further be 3.1# to 5.8#, such as 3.1#, 3.3#, 3.5#, 3.7#, 3.8#, 4.1#, 4.2#, 4.5# or 5.8#.

[0089] In some optional embodiments, the acid value of the biomass-based resin is 50 mgKOH / g to 500 mgKOH / g, such as 50 mgKOH / g, 100 mgKOH / g, 150 mgKOH / g, 200 mgKOH / g, 250 mgKOH / g, 300 mgKOH / g, 350 mgKOH / g, 400 mgKOH / g, 450 mgKOH / g or 500 mgKOH / g, etc., and may also be other values ​​within the range of 50 mgKOH / g to 500 mgKOH / g. In some typical embodiments, the acid value of the biomass-based resin is 50 mgKOH / g~150 mgKOH / g, and can further be 52 mgKOH / g~93 mgKOH / g, such as 52 mgKOH / g, 56 mgKOH / g, 60 mgKOH / g, 70 mgKOH / g, 77 mgKOH / g, 83 mgKOH / g, 84 mgKOH / g, 85 mgKOH / g or 93 mgKOH / g, etc.

[0090] In some optional embodiments, the iodine value of the biomass-based resin is 10gI2 / 100g~300gI2 / 100g, such as 10gI2 / 100g, 50gI2 / 100g, 100gI2 / 100g, 150gI2 / 100g, 200gI2 / 100g, 250gI2 / 100g or 300gI2 / 100g, etc., or it can be other values ​​within the range of 10gI2 / 100g~300gI2 / 100g. In some typical embodiments, the iodine value of the biomass-based resin is 70gI2 / 100g~180gI2 / 100g, and can further be 98gI2 / 100g~166gI2 / 100g, such as 98gI2 / 100g, 108gI2 / 100g, 125gI2 / 100g, 126gI2 / 100g, 133gI2 / 100g, 135gI2 / 100g, 137gI2 / 100g, 140gI2 / 100g, 153gI2 / 100g, 155gI2 / 100g or 166gI2 / 100g, etc.

[0091] In addition, the present invention also provides a composite material, and the raw materials for preparing the composite material include a rubber material and the above-mentioned biomass-based resin.

[0092] In some optional embodiments, the rubber material may include at least one of natural rubber, synthetic rubber and elastomer. In some more typical embodiments, the rubber material includes at least one of butadiene rubber (BR), styrene butadiene rubber (SBR), natural rubber (NR) and SBC elastomer.

[0093] The biomass-based resin provided by the present invention has an excellent elastic modulus-enhancing effect on elastomers such as SBR.

[0094] Furthermore, the present invention also provides the use of the composite material in automobile parts, packaging materials or electronic equipment.

[0095] The above-mentioned automobile parts and accessories may exemplarily but not limitatively include automobile tires, automobile interior decorations or automobile anti-damping parts, etc. Among them, automobile tires include but are not limited to tire treads, carcasses, sidewalls or inner tubes, etc.

[0096] The features and performance of the present invention are further described in detail below in conjunction with the embodiments.

[0097] The preparation method of the modified phosphotungstic acid catalyst used in the following examples and comparative examples is as follows: Step (1): Add phosphotungstic acid, soluble cesium salt (cesium chloride) and water into a closed, stirred high-pressure reactor and stir thoroughly; Step (2): Add the pre-dried carriers (H-ZMS-5 and SBA-15, respectively) into the reactor and soak at 25°C for 3 hours to form a stable chemical bond between the phosphotungstic acid and the carrier; Step (3): After the impregnation equilibrium, the remaining liquid is removed, and the catalyst is dried in a vacuum oven at 90° C. for 12 h to obtain a modified phosphotungstic acid catalyst.

[0098] Some information of each modified phosphotungstic acid catalyst is shown in Table 1.

[0099] Table 1 Modified phosphotungstic acid catalyst information

[0100] Example 1 This embodiment provides a biomass-based resin, referring to Figure 1 , and its preparation method is as follows: S1: In a high-pressure reactor R101 with stirring and nitrogen protection, decalin accounting for 40% of the total material mass is pre-added as the first solvent, cyclopentadiene (CPD) and norbornene (VN) are fully mixed in a mass ratio of 1:1 and added into the high-pressure reactor R101, and thermal free radical polymerization is carried out at 175°C and 0.25MPa for 2.0h; then divinyl ether (DE) accounting for 1.5% of the total material mass is added, and the reaction is continued at 200°C and 0.25MPa for 8h to obtain a first polymerization liquid.

[0101] S2: The first polymerization liquid is transported to a flash tower T101, and the first solvent and unreacted monomers are removed under the conditions of a pressure of 40 kPa and a temperature of 235°C. The light component obtained at the top of the flash tower T101 is passed into a microporous membrane separator M101, and the decahydronaphthalene separated in the microporous membrane separator M101 is recycled to the reactor R101; a cycloolefin copolymer with a Gardner color number of 2.0#, a melt viscosity (@40°C) of 1250 mPa·s, and a Z-average molecular weight of 880 is obtained in the reactor of the flash tower T101.

[0102] S3: The above-mentioned cycloolefin copolymer is pre-transported into a packed tower T102 (the packing in the packed tower T102 is composed of α-alumina and diatomaceous earth in a volume ratio of 1:0.3) to remove impurities by filtration, and then the cycloolefin copolymer is uniformly mixed with dehydroabietic acid and a second solvent (the mass ratio of methylcyclohexane to benzene is 1:1) in a mass ratio of 1:0.8:2, and then sent to a fixed bed reactor R102 loaded with a catalyst (II), and reacted at 100°C and 0.15 MPa for a residence time of 1.0 h to obtain a second polymerization liquid.

[0103] S4: The second polymerization liquid is passed into the alcohol washing kettle V101, and methanol accounting for 20% of the mass of the second polymerization liquid is added to elute the unreacted monomers. Then the second polymerization liquid enters the distillation tower T103, and the second solvent and oligomers are removed under the conditions of pressure of 40 kPa and temperature of 250°C to obtain a biomass-based resin with a softening point of 98°C, a Gardner color number of 4.0#, an acid value of 75 mgKOH / g, and an iodine value of 140 gI2 / 100g.

[0104] Example 2 The present embodiment provides a biomass-based resin, and the preparation method thereof differs from that of the embodiment 1 only in that the following conditions of step S3 are different: the cycloolefin copolymer after impurities are removed is uniformly mixed with 2,2-dimethylsuccinic anhydride and a second solvent (the mass ratio of methylcyclohexane to benzene is 1:1) at a mass ratio of 1:0.5:2.5, and then introduced into a fixed bed reactor R102 loaded with a catalyst (I), and reacted at 850°C and 0.12MPa for a residence time of 1.0h to obtain a second polymerization liquid.

[0105] Example 3 This embodiment provides a biomass-based resin, and the preparation method thereof is different from that of Embodiment 2 only in that the catalyst used in step S3 is different. The catalyst used in this embodiment is catalyst (II).

[0106] Example 4 This embodiment provides a biomass-based resin, and the preparation method thereof is different from that of Embodiment 2 only in that the catalyst used in step S3 is different. The catalyst used in this embodiment is catalyst (III).

[0107] Example 5 This embodiment provides a biomass-based resin, and the preparation method thereof is different from that of Embodiment 2 only in that the catalyst used in step S3 is different. The catalyst used in this embodiment is catalyst (IV).

[0108] Example 6 This embodiment provides a biomass-based resin. The preparation method thereof is different from that of embodiment 2 only in that the catalyst used in step S3 is different. The catalyst used in this embodiment is a phosphotungstic acid catalyst that has not been modified with Cs, namely catalyst V, and its molecular formula is H3PW 12 O 40 / H-ZMS-5, the active component content is 30%.

[0109] The differences between the above-mentioned Examples 2 to 6 and the performance results of the biomass-based resins prepared from each are shown in Table 2.

[0110] Table 2 Effects of different modified phosphotungstic acid catalysts on the properties of biomass-based resins

[0111] It can be seen from Table 2 that the different modified tungsten phosphate catalysts provided in Examples 2 to 5 of the present invention can increase the catalytic polymerization activity of bio-based carboxylic acid and cycloolefin copolymers, improve the softening point and acid value of the product, and reduce the iodine value of the product. However, as the acid value of the product increases, its color will also deepen to a certain extent. The tungsten phosphate catalyst used in Example 6, which is not modified with Cs, can also increase the softening point and acid value of the product to a certain extent and reduce the iodine value of the product.

[0112] Example 7 This embodiment provides a biomass-based resin, and the preparation method thereof is as follows: S1: In a high-pressure reactor R101 with stirring and nitrogen protection, decalin accounting for 35% of the total material mass is pre-added as the first solvent, cyclopentadiene (CPD) and 5-vinyl-2-norbornene (VNB) are fully mixed in a mass ratio of 1:0.5 and added into the high-pressure reactor R101, and thermal free radical polymerization is carried out at 200°C and 0.25MPa for 2.0h; then divinyl ether (DE) accounting for 1.5% of the total material mass is added, and the reaction is continued at 145°C and 0.18MPa for 10.0h to obtain a first polymerization liquid.

[0113] S2: The steps and conditions are the same as those in Example 1. The information of the obtained cycloolefin copolymer is shown in Table 3.

[0114] S3: The cycloolefin copolymer after impurities are removed is uniformly mixed with ricinoleic acid and a second solvent (the mass ratio of methylcyclohexane to benzene is 1:1) at a mass ratio of 1:0.5:2.5, and then introduced into a fixed bed reactor R102 loaded with a catalyst (III), and reacted at 85°C and 0.12 MPa for a residence time of 1.0 h to obtain a second polymerization liquid.

[0115] S4: The steps and conditions are the same as those in Example 1. The information of the obtained biomass-based resin is shown in Table 3.

[0116] Example 8 This embodiment provides a biomass-based resin, and the preparation method thereof is different from that of Example 7 only in that the mass ratio of CPD to VNB and the amount of DE used in step S1 are different. In this embodiment, the mass ratio of CPD to VNB is 1:1, and the amount of DE used is 1.5% of the total material mass.

[0117] Example 9 This embodiment provides a biomass-based resin, and the preparation method thereof is different from that of Example 7 only in that the mass ratio of CPD to VNB and the amount of DE used in step S1 are different. In this embodiment, the mass ratio of CPD to VNB is 1:1, and the amount of DE used is 3% of the total material mass.

[0118] Example 10 This embodiment provides a biomass-based resin, and the preparation method thereof is different from that of Example 7 only in that the mass ratio of CPD to VNB and the amount of DE used in step S1 are different. In this embodiment, the mass ratio of CPD to VNB is 1:1.5, and the amount of DE used is 3% of the total material mass.

[0119] Comparative Example 1 This comparative example provides a biomass-based resin, and the preparation method thereof is different from that of Example 7 only in that the mass ratio of CPD to VNB and the amount of DE used in step S1 are different. In this example, the mass ratio of CPD to VNB is 1:1, and DE is not used.

[0120] The differences between the above-mentioned Examples 7 to 10 and Comparative Example 1 and the performance results of the cycloolefin copolymers and biomass-based resins prepared from them are shown in Table 3.

[0121] Table 3 Effects of different raw material ratios on the properties of cycloolefin copolymers and biomass-based resins

[0122] As can be seen from Table 3, in Examples 7 to 10 of the present invention, in the free radical polymerization of the cycloolefin copolymer, the cyclopentadiene and norbornene monomers are first subjected to the Diels-Alder reaction to generate cyclic molecules, and then a proper amount of divinyl ether is added as a molecular weight regulator, thereby obtaining a liquid cycloolefin copolymer with low viscosity and low Z-average molecular weight.

[0123] The performance of the copolymers of cycloolefin copolymers with different physical and chemical properties using modified phosphotungstic acid catalysts and bio-based carboxylic acids includes: 1) The changes in molecular weight and melt viscosity of cycloolefin copolymers have little effect on the acid value properties of modified tear-resistant resins, that is, the content of carboxylic acid groups in the product molecules is mainly related to the modified bio-based carboxylic acid monomer, dosage and process conditions, but has nothing to do with the base resin; 2) As the molecular weight and melt viscosity increase, the softening point of the modified tear-resistant resin increases and the iodine value decreases, that is, different cycloolefin copolymers can affect the saturation and internal structure of the copolymer product, and will further affect its application performance; 3) The catalytic copolymerization efficiency of cycloolefin copolymers prepared without adding divinyl ether monomers and bio-based carboxylic acids is low, and the overall acid value and iodine value are significantly reduced.

[0124] Embodiment 11 The present embodiment provides a biomass-based resin, and the preparation method thereof differs from that of Example 1 only in that the following conditions of step S3 are different: the cycloolefin copolymer after impurities are removed is uniformly mixed with 2,5-furandicarboxylic acid and a second solvent (the mass ratio of methylcyclohexane to benzene is 1:1) at a mass ratio of 0.5:1:2, and then introduced into a fixed bed reactor R102 loaded with a catalyst (IV), and reacted at 100°C and 0.12 MPa for a residence time of 1.0 h to obtain a second polymerization liquid.

[0125] Example 12 This embodiment provides a biomass-based resin, and the preparation method thereof is different from that of Embodiment 11 only in that the bio-based carboxylic acid used in step S3 is rosin acid.

[0126] Example 13 This embodiment provides a biomass-based resin, and the preparation method thereof is different from that of Embodiment 11 only in that the bio-based carboxylic acid used in step S3 is allyl succinic anhydride.

[0127] Comparative Example 2 This comparative example provides a biomass-based resin, the preparation method of which is different from that of Example 11 only in that no bio-based carboxylic acid is used in step S3.

[0128] The differences between the above-mentioned Examples 11 to 13 and Comparative Example 2 and the performance results of the biomass-based resins prepared from each are shown in Table 4.

[0129] Table 4 Effects of different bio-based carboxylic acids on the properties of biomass-based resins

[0130] It can be seen from Table 4 that the copolymerization product of cycloolefin copolymer and bio-based carboxylic acid has greatly improved softening point, acid value and iodine value and polarity compared with the unmodified resin (Comparative Example 2), which helps it to play a reinforcing role in rubber and elastomers. At the same time, modifying cycloolefin copolymer with different bio-based carboxylic acids will obtain biomass-based resins with differentiated molecular structures and functions, which helps to improve compatibility with substrates of different polarity and expand the application field.

[0131] Comparative Example 3 This comparative example provides a biomass-based resin, and its preparation method is as follows: S1: Same as Example 1.

[0132] S2: Same as Example 1.

[0133] S3: Same as Example 1.

[0134] S4: The second polymer solution is passed into a distillation tower T103 to remove the solvent and oligomers at a pressure of 40 kPa and 250°C to obtain a biomass-based resin having a softening point of 104.5°C, a Gardner color number of 9.0#, an acid value of 945 mgKOH / g, and an iodine value of 132 gI2 / 100g.

[0135] It can be seen from Comparative Example 3 that, before distillation, if organic alcohol is not used to elute the unreacted monomers, the properties of the final biomass-based resin, such as the Gardner color number and the acid value, will deteriorate.

[0136] Comparative Example 4 This comparative example provides a biomass-based resin, and the preparation method thereof is different from that of Example 1 only in that the second solvent used in step S3 is different. This example uses methylcyclohexane as the single solvent.

[0137] Comparative Example 5 This comparative example provides a biomass-based resin, and the preparation method thereof is different from that of Example 1 only in that the second solvent used in step S3 is different. This example uses toluene as the single solvent.

[0138] Table 5 Effect of single second solvent on the properties of biomass-based resin

[0139] It can be seen from Table 5 that the use of a single-component second solvent can also obtain a biomass-based resin with a certain acid value and iodine value, but its acid grafting rate is lower than that of the composite solvent, and when toluene is used as the second solvent, the softening point of the product is significantly reduced and the color is deepened.

[0140] Application Examples This application example provides 5 rubber composition samples, corresponding to a blank group, experimental group 1, experimental group 2, experimental group 3 and a control group, respectively. The formula of the rubber composition of each group is shown in Table 6.

[0141] Among them, the biomass resin used in experimental group 1 is the biomass-based resin prepared in Example 11, the biomass resin used in experimental group 2 is the biomass-based resin prepared in Example 12, the biomass resin used in experimental group 3 is the biomass-based resin prepared in Example 13, and the biomass resin used in the control group is the biomass-based resin prepared in Comparative Example 2.

[0142] Table 6 Rubber composition formula

[0143] Here, "phr" refers to the mass parts of the additive per 100 parts of rubber.

[0144] The rubber compositions of the above groups were subjected to three-stage pre-vulcanization, and the vulcanization conditions were 153°C×25min, 153°C×35min, and 153°C×50min.

[0145] After vulcanization treatment, the following performance tests are carried out, and the measurement conditions include: The tear strength is tested in accordance with the method specified in GB / T529 "Determination of tear strength of vulcanized rubber or thermoplastic rubber (trouser-shaped, right-angled and crescent-shaped test specimens)"; 300% tensile stress, 100% tensile stress, tensile strength and elongation at break are tested in accordance with the method specified in GB / T528 "Determination of tensile stress-strain properties of vulcanized rubber or thermoplastic rubber"; hardness is tested in accordance with the method specified in GB / T6031; Mooney viscosity ML (1+4) 100℃ is tested in accordance with the method specified in GB / T1232.1; Mooney scorch time is tested in accordance with the method specified in GB / T1233.

[0146] The measurement results are shown in Tables 7 and 8.

[0147] Table 7 Physical properties of rubber composition

[0148] Table 8 Mooney viscosity and Mooney scorch time

[0149] It can be seen from Tables 7 and 8 that the biomass-based resin prepared by Examples 11 to 13 of the present invention, which were sequentially added with 3phr of the rubber compositions in Experimental Groups 1 to 3, had greatly enhanced tear strength and elongation at break before and after vulcanization, and the application properties such as 300% tensile stress, 100% tensile stress and tensile strength were also improved to a certain extent. At the same time, at the initial stage of vulcanization, after adding the tear-resistant resin, the Mooney viscosity ML (1+4) at 100°C was generally smaller than that of the rubber composition without the addition, and the Mooney scorch time was shortened, showing better processing performance.

[0150] The biomass-based resin used in the control group, because it was not modified with bio-based carboxylic acid, showed varying degrees of degradation in its physical and chemical properties in the rubber composition application test.

[0151] As mentioned above, the biomass-based resin provided in the embodiment of the present invention can significantly improve the tear resistance and chipping resistance of the rubber, can effectively increase the viscosity of the rubber and has good compatibility with rubber, and the biomass-based resin provided in the embodiment of the present invention also has good dynamic properties and a high modulus, which helps to improve the cut resistance of the tread rubber and improve the processing performance of the rubber compound.

[0152] In summary, the novel medium- and low-molecular-weight bio-based synthetic resin obtained by catalytic copolymerization of bio-based organic carboxylic acid and cycloolefin provided by the present invention has excellent viscosity-increasing performance, is suitable for modification of butadiene rubber (BR), styrene-butadiene rubber SBR, natural rubber NR, SBC elastomer, etc., can improve the tear resistance of composite materials, and can be applied to automotive parts (including rubber tires, automotive interiors, automotive anti-damping parts, etc.), packaging materials or electronic equipment and other fields.

Claims

1. A method for preparing a biomass-based resin, characterized in that: The following steps are involved: Conducting a thermal free radical polymerization reaction of cyclopentadiene and its derivatives with norbornene monomers in the presence of a first solvent, and then adding a linear ether compound to continue the reaction to obtain a first polymerization solution containing a cycloolefin copolymer; The cyclic olefin copolymer in the first polymerization solution is separated, and the separated cyclic olefin copolymer is reacted with a bio-based carboxylic acid in the presence of a second solvent and a catalyst to obtain a biomass-based resin.

2. The preparation method according to claim 1, characterized in that: The preparation of the first polymer solution includes at least one of the following features: Feature 1: The temperature of the thermal free radical polymerization reaction is 100°C~250°C, the pressure is 0.15MPa~2.0MPa, and the time is 0.5h~5.0h; Feature 2: The mass ratio of the cyclopentadiene and its derivatives to the norbornene monomer is 1:0.1 to 1:2.0; Feature 3: The first solvent accounts for 15% to 50% of the total material mass, and the total material is the sum of the cyclopentadiene and its derivatives, the norbornene monomers and the linear ether compounds; Feature 4: After adding the linear ether compound, the temperature for continuing the reaction is 100°C to 250°C, the pressure is 0.15MPa to 2.0MPa, and the time is 1.0h to 10h; Feature 5: The amount of the linear ether compound added is 0.1% to 5% of the total material mass, and the total material is the sum of the cyclopentadiene and its derivatives, the norbornene monomers and the linear ether compound; Feature 6: The cyclopentadiene and its derivatives include at least one of cyclopentadiene, methylcyclopentadiene, dimethylcyclopentadiene, dicyclopentadiene, methylcyclopentadiene dimer and cyclopentadiene-methylcyclopentadiene dimer; Feature 7: The norbornene monomer includes at least one of norbornene, 2,5-norbornadiene, 5-vinyl-2-norbornene, 5-ethylidene-2-norbornene and 2-allyl-5-norbornene; Feature 8: The first solvent includes decahydronaphthalene; Feature 9: The linear ether compound includes a divinyl ether monomer.

3. The preparation method according to claim 1, characterized in that: Separating the cyclic olefin copolymer in the first polymer solution comprises at least one of the following features: Feature 10: Separating the cycloolefin copolymer in the first polymerization solution by flash evaporation; wherein the flash evaporation pressure is 20 kPa to 80 kPa, and the flash evaporation temperature is 180° C. to 250° C.; Feature 11: The isolated cycloolefin copolymer has a Gardner color number of ≤4.0#, a melt viscosity at 40°C of ≤3000 mPa·s, and a Z-average molecular weight of ≤1500.

4. The preparation method according to claim 1, characterized in that: The reaction of the cyclic olefin copolymer and the bio-based carboxylic acid includes at least one of the following features: Feature 12: The reaction temperature of the cyclic olefin copolymer and the bio-based carboxylic acid is 50° C. to 120° C., the reaction pressure is 0.1 MPa to 1.0 MPa, and the reaction time is 0.25 h to 2.0 h; Feature 13: The mass ratio of the cyclic olefin copolymer to the bio-based carboxylic acid and the second solvent is 1:(0.7-1.5):(0.75-10) respectively; Feature 14: The bio-based carboxylic acid includes at least one of 3-hydroxypropionic acid, 2,5-furandicarboxylic acid, abietic acid, dehydroabietic acid, dehydroabietic acid, 2,2-dimethylsuccinic anhydride, allylsuccinic anhydride, butylsuccinic anhydride, 2-octenylsuccinic anhydride, ricinoleic acid, dehydrated ricinoleic acid, itaconic acid and hexylitaconic acid; Feature 15: The second solvent includes benzene, cyclohexane and its derivatives; Feature 16: The catalyst comprises a phosphotungstic acid catalyst; Feature 17: The reaction of the cyclic olefin copolymer and the bio-based carboxylic acid is carried out in a fixed bed reactor.

5. The preparation method according to any one of claims 1 to 4, characterized in that First, the separated cyclic olefin copolymer is freed of impurities in a packed tower, and then reacted with the bio-based carboxylic acid and the second solvent in the presence of the catalyst; Wherein, the filler used in the packed tower includes at least one of α-alumina and diatomaceous earth.

6. The preparation method according to any one of claims 1 to 4, characterized in that Also includes: post-treating a second polymerization solution obtained by reacting the cyclic olefin copolymer with the bio-based carboxylic acid; The post-treatment includes: removing the unreacted monomers and the remaining solvent and oligomers in the second polymerization solution; wherein, the unreacted monomers are eluted with organic alcohol, and the remaining solvent and oligomers are removed by distillation.

7. The preparation method according to any one of claims 1 to 4, characterized in that Also includes: Recovering the light component remaining after separating the cycloolefin copolymer from the first polymerization liquid to obtain the first solvent in the light component; Wherein, recovering the light component comprises at least one of the following characteristics: Feature 18: Using a microporous membrane to separate the light component; Feature 19: The separation of the light component is carried out under the conditions of 15°C ~ 35°C and 0.1MPa ~ 0.3MPa.

8. A biomass-based resin, characterized in that The biomass-based resin is prepared by the preparation method according to any one of claims 1 to 7; The biomass-based resin has at least one of the following characteristics: Feature 20: The softening point of the biomass-based resin is 80°C to 140°C; Feature 21: The Gardner color number of the biomass-based resin is ≤8#; Feature 22: The acid value of the biomass-based resin is 50 mgKOH / g to 500 mgKOH / g; Feature 23: The iodine value of the biomass-based resin is 10gI2 / 100g~300gI2 / 100g.

9. A composite material, characterized in that: The raw materials for preparing the composite material include a rubber material and the biomass-based resin according to claim 7 or 8.

10. Use of the composite material according to claim 9 in automobile parts, packaging materials or electronic devices.

Citation Information

Patent Citations

  • Resin for improving rubber tear resistance, preparation method and application of resin

    CN105254854A

  • Rosin modified C9 petroleum resin, preparation method and application thereof

    CN106967201A

  • Preparation method of BOPP film stiffening agent

    CN113717486A

  • Tear-resistant resin, preparation method thereof and rubber composition containing resin

    CN114907570A

  • Biomass group-containing polar polyolefin copolymer and preparation method thereof

    CN115926032A