Flexible water-based light-cured resin and preparation method thereof

By introducing flexible aqueous silicone crosslinked monomers containing hydrophilic carboxyl and alkyl long chains into UV cured polyurethane, the problem of insufficient water resistance and wear resistance of polyurethane is solved, and the polyurethane is improved in the aqueous resin. Dispersibility and mechanical properties.

CN119081015AInactive Publication Date: 2024-12-06JIANG OMAHA NEW MATERIALS CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411145752.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

UV cured polyurethane has low water resistance, poor toughness and poor wear resistance, especially in water-based resin emulsions, which affects its performance.

Method used

Flexible aqueous silicone crosslinking monomers are prepared by acid chloride esterification reaction and acid anhydride ring-opening esterification reaction to prepare flexible aqueous silicone crosslinking monomers containing hydrophilic carboxyl and alkyl long chains, combined with aqueous polyurethane acrylic acid The ester is photocured to improve its crosslinking and dispersion.

Benefits of technology

The toughness, elongation of break and water resistance of polyurethane film are significantly improved, the water absorption and mass loss rate are reduced, and the hardness and wear resistance are enhanced.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081015A_ABST
    Figure CN119081015A_ABST
Patent Text Reader

Abstract

The invention belongs to the technical field of light-cured resins, and discloses a flexible water-based light-cured resin and a preparation method thereof, and the flexible water-based light-cured resin comprises 100 parts by weight of water-based polyurethane acrylate, 2.4-3 parts by weight of a photoinitiator, 4-9 parts by weight of a reactive diluent, 3-12 parts by weight of a flexible water-based siloxane crosslinking monomer, 0.4-0.8 part by weight of an antifoaming agent, and 0.6-0.8 part by weight of an emulsifier. 0.3 to 1.2 parts by weight of a neutralizer; the flexible water-based siloxane crosslinking monomer disclosed by the invention contains two alkenyl groups, can replace part of reactive diluents, and is subjected to photocuring crosslinking reaction with polyurethane acrylate, so that flexible alkyl long chains and siloxane groups are grafted into polyurethane, and the hardness, tensile property, water resistance and wear resistance of the polyurethane are improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of photocurable resins, and in particular relates to a flexible water-based photocurable resin and a preparation method thereof. Background Art

[0002] Polyurethane acrylate is a new type of polyurethane resin containing active olefin groups. Under the action of photoinitiators, it can undergo photocuring reaction with active diluents. It has a fast curing speed and little environmental pollution. It can be made into photocurable coatings and photocurable inks, etc., and is widely used in printed circuit boards, electronic components, medical supplies, etc. Improving the toughness, water resistance, wear resistance and other properties of polyurethane acrylate can expand its practical application areas.

[0003] Modification of polyurethane with organosilicon substances can improve its flexibility, wear resistance, water resistance and other properties; Patent No. CN112225901B discloses the use of trimethylolpropane, castor oil, diisocyanate, hydroxyethyl acrylate and the like as raw materials to prepare polyurethane acrylate, which is then photocured with octavinyl polyhedral oligomeric silsesquioxane to obtain a photocurable polyurethane acrylate having the advantages of high hardness, good mechanical properties, hydrolysis resistance and the like. However, the octavinyl polyhedral oligomeric silsesquioxane does not contain a hydrophilic group, and has poor water solubility and dispersibility in the water-based resin emulsion, which will affect the performance of the water-based resin. Summary of the invention

[0004] The invention solves the problems of low water resistance, poor toughness and poor wear resistance of UV-cured polyurethane.

[0005] The technical solution of the present invention is a flexible water-based photocurable resin, which comprises 100 parts by weight of water-based polyurethane acrylate, 2.4-3 parts by weight of photoinitiator, 4-9 parts by weight of active diluent, 3-12 parts by weight of flexible water-based siloxane cross-linking monomer, 0.4-0.8 parts by weight of defoamer, 0.6-0.8 parts by weight of emulsifier, and 0.3-1.2 parts by weight of neutralizer.

[0006] The preparation method of the flexible water-based siloxane cross-linking monomer is as follows: add methyl methacrylate alkyl ester and siloxane dianhydride compound to the solvent, heat to 100-110°C, stir and condense reflux reaction for 6-10 hours, distill the solution under reduced pressure, wash with petroleum ether and acetone in turn, and dry to obtain a flexible water-based siloxane cross-linking monomer.

[0007] The structural formula of methacrylate alkyl ester is as follows ; n is 9, 10, 11, 12, 13.

[0008] The structural formula of siloxane dianhydride compound is as follows: .

[0009] Furthermore, the photoinitiator is diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide; and the active diluent is tripropylene glycol diacrylate or dipropylene glycol diacrylate.

[0010] Furthermore, the defoaming agent is an organosilicon defoaming agent; the emulsifier is a polyether-modified silicone oil emulsifier; and the neutralizing agent is triethylamine.

[0011] Furthermore, in the method for preparing the flexible water-based siloxane cross-linking monomer, the solvent is toluene or 1,4-dioxane.

[0012] Furthermore, in the preparation method of the flexible water-based siloxane cross-linking monomer, the molar ratio of methacrylate alkyl ester to siloxane dianhydride compound is (1.9-2.1):1.

[0013] Furthermore, the preparation method of methacrylic acid alkyl ester is as follows: add methacrylic acid glycidyl ester, alkyl acid, catalyst, and inhibitor in a molar ratio of 1: (1-1.1): (0.0038-0.0045): (0.005-0.006) to 1,4-dioxane, heat to 90-100°C, stir and condense reflux to react for 4-8 hours, remove low boiling points by vacuum distillation, add water and dichloromethane, shake and separate the layers, extract and separate, dry the organic phase to remove water, vacuum distill, wash with petroleum ether, and dry to obtain methacrylic acid alkyl ester.

[0014] Furthermore, the alkyl acid is decanoic acid, undecanoic acid, dodecanoic acid, tridecanoic acid or tetradecanoic acid; the catalyst is tetrabutylammonium bromide or triphenylphosphine; and the inhibitor is 4-methoxyphenol.

[0015] Furthermore, the preparation method of the siloxane dianhydride compound is: in an ice bath, 1,3-bis(3-hydroxypropyl)-1,1,3,3-tetramethyldisiloxane, triethylamine, and trimellitic anhydride chloride in a molar ratio of 1:(2-2.2):(2-2.2) are added to dichloromethane, followed by reaction at room temperature for 5-8 hours, vacuum distillation, washing with water, drying, and recrystallization in ethyl acetate to obtain the siloxane dianhydride compound.

[0016] Furthermore, the preparation method of the flexible water-based photocurable resin is: adding water-based polyurethane acrylate, reactive diluent, flexible water-based siloxane cross-linking monomer, defoamer, emulsifier, neutralizer into water, stirring and mixing, and then adding photoinitiator to obtain the flexible water-based photocurable resin.

[0017] Technical effect of the invention: The invention utilizes 1,3-bis(3-hydroxypropyl)-1,1,3,3-tetramethyldisiloxane and trimellitic anhydride chloride to carry out an acyl chloride esterification reaction to obtain a siloxane dianhydride compound, which is then subjected to an anhydride ring-opening esterification reaction with the hydroxyl group of methacrylate alkyl ester to obtain a novel flexible water-based siloxane cross-linking monomer containing a hydrophilic carboxyl group, a flexible siloxane and an alkyl long chain.

[0018] The flexible water-based siloxane cross-linking monomer of the present invention contains multiple hydrophilic carboxyl groups, has good dispersibility in water-based polyurethane acrylate emulsion, and contains two alkenyl groups, which can replace part of the active diluent, and undergo a photocuring cross-linking reaction with polyurethane acrylate, thereby grafting flexible alkyl long chains and siloxane groups into polyurethane, and can also improve the toughness and elongation at break of the film, and the flexible water-based siloxane cross-linking monomer undergoes a cross-linking reaction with polyurethane acrylate, which improves the cross-linking degree of the polyurethane molecular chain, is conducive to reducing the water absorption rate of the film, and improves its water resistance. At the same time, the polyurethane film containing the siloxane structure has higher hardness, lower mass loss rate, and better wear resistance. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 It is the reaction formula for preparing alkyl methacrylate.

[0020] Figure 2 It is the reaction formula for preparing siloxane dianhydride compounds.

[0021] Figure 3 It is a reaction formula for preparing flexible waterborne siloxane cross-linking monomers. DETAILED DESCRIPTION

[0022] The following are specific embodiments of the present invention, and the embodiments are intended to further describe the present invention rather than to limit the present invention.

[0023] The waterborne polyurethane acrylate of the invention has a brand name of Laromer-UA 9135Aqua; the organic silicon defoamer has a brand name of TEGO810; and the 0.6-0.8g emulsifier polyether modified silicone oil has a brand name of DY-ET123.

[0024] Example 1 To 20 mL of 1,4-dioxane, add 10 mmol of glycidyl methacrylate, 10 mmol of n-decanoic acid, 0.038 mmol of catalyst tetrabutylammonium bromide, and 0.05 mmol of inhibitor 4-methoxyphenol, heat to 100°C, stir and condense under reflux for 4 hours, remove low boiling points by distillation under reduced pressure, add water and dichloromethane, shake and separate the layers, extract and separate, dry the organic phase to remove water, distill under reduced pressure, wash with petroleum ether, and dry to obtain methacrylic acid alkyl ester.

[0025] In an ice bath, add 4 mmol 1,3-bis(3-hydroxypropyl)-1,1,3,3-tetramethyldisiloxane, 8 mmol triethylamine, and 8 mmol trimellitic anhydride chloride to 25 mL dichloromethane, then react at room temperature for 5 h, distill under reduced pressure, wash with water, dry and recrystallize in ethyl acetate to obtain a siloxane dianhydride compound.

[0026] Add 20 mmol of methyl methacrylate and 10 mmol of siloxane dianhydride compound to 80 mL of toluene solvent, heat to 100°C, stir and condense under reflux for 10 hours, distill the solution under reduced pressure, wash with petroleum ether and acetone in turn, and dry to obtain a flexible water-based siloxane cross-linking monomer.

[0027] To 80 mL of water, add 100 g of waterborne polyurethane acrylate, 9 g of active diluent dipropylene glycol diacrylate, 3 g of flexible waterborne siloxane crosslinking monomer, 0.5 g of silicone defoamer, 0.8 g of emulsifier polyether modified silicone oil, and 0.3 g of neutralizer triethylamine, stir to mix, and then add 3 g of photoinitiator diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a flexible waterborne light-curable resin.

[0028] Example 2 To 30 mL of 1,4-dioxane, add 10 mmol of glycidyl methacrylate, 11 mmol of dodecanoic acid, 0.038 mmol of catalyst triphenylphosphine, and 0.06 mmol of inhibitor 4-methoxyphenol, heat to 100°C, stir and reflux for 5 hours, remove low boiling points by distillation under reduced pressure, add water and dichloromethane, shake and separate the layers, extract and separate, dry the organic phase to remove water, distill under reduced pressure, wash with petroleum ether, and dry to obtain methacrylic acid alkyl ester.

[0029] In an ice bath, add 4 mmol 1,3-bis(3-hydroxypropyl)-1,1,3,3-tetramethyldisiloxane, 8 mmol triethylamine, and 8 mmol trimellitic anhydride chloride to 20 mL dichloromethane, then react at room temperature for 6 h, distill under reduced pressure, wash with water, dry and recrystallize in ethyl acetate to obtain a siloxane dianhydride compound.

[0030] Add 21 mmol of methyl methacrylate and 10 mmol of siloxane dianhydride to 80 mL of 1,4-dioxane solvent, heat to 100°C, stir and condense under reflux for 6 hours, distill the solution under reduced pressure, wash with petroleum ether and acetone in turn, and dry to obtain a flexible water-based siloxane cross-linking monomer.

[0031] To 80 mL of water, add 100 g of waterborne polyurethane acrylate, 9 g of active diluent tripropylene glycol diacrylate, 3 g of flexible waterborne siloxane crosslinking monomer, 0.4 g of silicone defoamer, 0.6 g of emulsifier polyether modified silicone oil, and 0.3 g of neutralizer triethylamine, stir to mix, and then add 2.4 g of photoinitiator diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a flexible waterborne light-curable resin.

[0032] Example 3 To 30 mL of 1,4-dioxane, add 10 mmol of glycidyl methacrylate, 10 mmol of tetradecanoic acid, 0.045 mmol of catalyst tetrabutylammonium bromide, and 0.06 mmol of inhibitor 4-methoxyphenol, heat to 90°C, stir and condense under reflux for 8 hours, remove low boiling points by distillation under reduced pressure, add water and dichloromethane, shake and separate the layers, extract and separate, dry the organic phase to remove water, distill under reduced pressure, wash with petroleum ether, and dry to obtain methacrylic acid alkyl ester.

[0033] In an ice bath, 4 mmol 1,3-bis(3-hydroxypropyl)-1,1,3,3-tetramethyldisiloxane, 8.8 mmol triethylamine, and 8.8 mmol trimellitic anhydride chloride were added to 25 mL dichloromethane, and then reacted at room temperature for 5 h. The mixture was distilled under reduced pressure, washed with water, dried, and recrystallized in ethyl acetate to obtain a siloxane dianhydride compound.

[0034] Add 19 mmol of methyl methacrylate and 10 mmol of siloxane dianhydride compound to 60 mL of toluene solvent, heat to 110°C, stir and condense under reflux for 6 hours, distill the solution under reduced pressure, wash with petroleum ether and acetone in turn, and dry to obtain a flexible water-based siloxane cross-linking monomer.

[0035] To 80 mL of water, add 100 g of waterborne polyurethane acrylate, 9 g of active diluent tripropylene glycol diacrylate, 3 g of flexible waterborne siloxane crosslinking monomer, 0.8 g of silicone defoamer, 0.8 g of emulsifier polyether modified silicone oil, and 0.3 g of neutralizer triethylamine, stir to mix, and then add 2.6 g of photoinitiator diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a flexible waterborne light-curable resin.

[0036] Comparative Example 1 The difference between this comparative example and Example 1 is that no flexible water-based siloxane cross-linking monomer is added to the photocurable resin.

[0037] To 80 mL of water, add 100 g of waterborne polyurethane acrylate, 9 g of active diluent dipropylene glycol diacrylate, 0.5 g of silicone defoamer, 0.8 g of emulsifier polyether modified silicone oil, and 0.3 g of neutralizer triethylamine, stir to mix, and then add 3 g of photoinitiator diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a flexible waterborne light-curable resin.

[0038] Comparative Example 2 The difference between this comparative example and Example 1 is that methacrylate alkyl ester is used instead of the flexible waterborne siloxane crosslinking monomer.

[0039] To 80 mL of water, add 100 g of waterborne polyurethane acrylate, 9 g of active diluent dipropylene glycol diacrylate, 3 g of flexible waterborne siloxane crosslinking monomer, 0.5 g of silicone defoamer, 0.8 g of emulsifier polyether modified silicone oil, and 0.3 g of neutralizer triethylamine, stir to mix, and then add 3 g of photoinitiator diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a flexible waterborne light-curable resin.

[0040] Comparative Example 3 The difference between this comparative example and Example 1 is that a siloxane dianhydride compound is used instead of the flexible water-based siloxane cross-linking monomer.

[0041] To 80 mL of water, add 100 g of waterborne polyurethane acrylate, 9 g of active diluent dipropylene glycol diacrylate, 3 g of flexible waterborne siloxane crosslinking monomer, 0.5 g of silicone defoamer, 0.8 g of emulsifier polyether modified silicone oil, and 0.3 g of neutralizer triethylamine, stir to mix, and then add 3 g of photoinitiator diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a flexible waterborne light-curable resin.

[0042] Pour the light-curing resin on the surface of the substrate and cure it in a UV curing machine for 60 seconds with a power of 3kW. After curing, the paint film is formed and the hardness of the paint film is tested according to the method of GB / T 6739-2022.

[0043] The photocurable resin is photocured to form a film. The tensile properties of the film are tested using a tensile testing machine according to the method of GB / T 528-2009.

[0044] The polyurethane film was dried to remove water, weighed, and soaked in water for 24 hours. After taking out the film, the excess water on the surface was wiped off, weighed, and the water absorption rate R was calculated. R = (m-m0) / m0×100%.

[0045] The polyurethane film sample was subjected to a ring-block wear test in a wear tester, with a 45# steel ring for rubbing, a load value of 19.6N, and a rotation speed of 200r / min. The wear resistance of the polyurethane film was evaluated by the method of weight loss per unit area. The block width L and the wear scar width d of the polyurethane film sample were measured, and the mass of the film sample before and after wear was weighed. The mass loss rate W was calculated.

[0046] W = (M0-M) / (L×d). M0 is the mass before wear and M is the mass after wear.

[0047] Table 1 Photocurable resin performance test

[0048] As shown in Table 1, compared with Comparative Example 1, Examples 1-3 add flexible waterborne siloxane crosslinking monomers, which contain two alkenyl groups and can replace part of the active diluents, and undergo a photocuring crosslinking reaction with polyurethane acrylate, thereby grafting flexible alkyl long chains and siloxane groups into polyurethane, and can also improve the toughness and elongation at break of the film. In addition, the flexible waterborne siloxane crosslinking monomers undergo a crosslinking reaction with polyurethane acrylate, which increases the crosslinking degree of the polyurethane molecular chain, helps to reduce the water absorption rate of the film, and improves its water resistance. At the same time, the polyurethane film containing the siloxane structure has higher hardness, lower mass loss rate, and better wear resistance.

[0049] Comparative Example 2 uses methyl methacrylate to replace the flexible water-based siloxane cross-linking monomer, which contains only one olefin group, has poor cross-linking performance with polyurethane acrylate, and does not contain siloxane groups, resulting in the polyurethane film having lower hardness, higher water absorption, lower mass loss rate, and poor water resistance and wear resistance.

[0050] Comparative Example 3 uses a siloxane dianhydride compound instead of a flexible water-based siloxane cross-linking monomer, which does not contain a hydrophilic carboxyl group, has poor dispersibility in an aqueous resin emulsion, and does not contain an olefin group, and cannot undergo a photocuring reaction with polyurethane acrylate. The siloxane dianhydride compound has poor compatibility with polyurethane acrylate, and the effect of adding it to the coating on improving its mechanical properties is low, and it does not exhibit good hardness, tensile properties, and wear resistance.

[0051] Example 4 To 80 mL of water, add 100 g of waterborne polyurethane acrylate, 7.5 g of active diluent dipropylene glycol diacrylate, 5 g of flexible waterborne siloxane crosslinking monomer, 0.5 g of silicone defoamer, 0.8 g of emulsifier polyether modified silicone oil, and 0.3 g of neutralizer triethylamine, stir to mix, and then add 3 g of photoinitiator diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a flexible waterborne light-curable resin.

[0052] Example 5 To 80 mL of water, add 100 g of waterborne polyurethane acrylate, 6 g of active diluent dipropylene glycol diacrylate, 7 g of flexible waterborne siloxane crosslinking monomer, 0.5 g of silicone defoamer, 0.8 g of emulsifier polyether modified silicone oil, and 0.3 g of neutralizer triethylamine, stir to mix, and then add 3 g of photoinitiator diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a flexible waterborne light-curable resin.

[0053] Example 6 To 80 mL of water, add 100 g of waterborne polyurethane acrylate, 5 g of active diluent dipropylene glycol diacrylate, 9.5 g of flexible waterborne siloxane crosslinking monomer, 0.5 g of silicone defoamer, 0.8 g of emulsifier polyether modified silicone oil, and 0.3 g of neutralizer triethylamine, stir to mix, and then add 3 g of photoinitiator diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a flexible waterborne light-curable resin.

[0054] Example 7 To 80 mL of water, add 100 g of waterborne polyurethane acrylate, 4 g of active diluent dipropylene glycol diacrylate, 12 g of flexible waterborne siloxane crosslinking monomer, 0.5 g of silicone defoamer, 0.8 g of emulsifier polyether modified silicone oil, and 0.3 g of neutralizer triethylamine, stir to mix, and then add 3 g of photoinitiator diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide to obtain a flexible waterborne light-curable resin.

[0055] The flexible water-based siloxane cross-linking monomers of Examples 4-7 were all prepared by the method of Example 1.

[0056] The flexible water-based photocurable resin was photocured according to the above method, and then the performance was tested.

[0057] Table 2 Performance test of flexible water-based photocurable resin

[0058] In Examples 4-7, at different ratios of reactive diluent and flexible waterborne siloxane crosslinking monomer, the flexible waterborne photocurable polyurethane resins all have relatively high hardness, excellent tensile properties, low water absorption and friction mass loss rate, and excellent water resistance and wear resistance.

[0059] The above are only several embodiments of the present application, and do not limit the present application in any form. Although the present application discloses the preferred embodiments as above, these embodiments are not used to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases, and all belong to the scope of the technical solution of the present application.

Claims

1. A flexible water-based photocurable resin, characterized in that: The composition comprises 100 parts by weight of waterborne polyurethane acrylate, 2.4-3 parts by weight of photoinitiator, 4-9 parts by weight of active diluent, 3-12 parts by weight of flexible waterborne siloxane crosslinking monomer, 0.4-0.8 parts by weight of defoamer, 0.6-0.8 parts by weight of emulsifier, and 0.3-1.2 parts by weight of neutralizer; The preparation method of the flexible waterborne siloxane crosslinking monomer is as follows: add methacrylic acid alkyl ester and siloxane dianhydride compound to a solvent, heat to 100-110° C., stir and condense reflux reaction for 6-10 hours, distill the solution under reduced pressure, wash with petroleum ether and acetone in sequence, and dry to obtain a flexible waterborne siloxane crosslinking monomer; The structural formula of the methacrylate ester is as follows ; n is 9, 10, 11, 12, 13; The structural formula of the siloxane dianhydride compound is as follows: 。 2. The flexible water-based photocurable resin according to claim 1, characterized in that: The photoinitiator is diphenyl-(2,4,6-trimethylbenzoyl)phosphine oxide; the active diluent is tripropylene glycol diacrylate or dipropylene glycol diacrylate.

3. The flexible water-based photocurable resin according to claim 1, characterized in that: The defoamer is an organic silicon defoamer; the emulsifier is a polyether modified silicone oil emulsifier; and the neutralizer is triethylamine.

4. The flexible water-based photocurable resin according to claim 1, characterized in that: In the method for preparing the flexible water-based siloxane cross-linking monomer, the solvent is toluene or 1,4-dioxane.

5. The flexible water-based photocurable resin according to claim 1, characterized in that: In the preparation method of the flexible water-based siloxane cross-linking monomer, the molar ratio of methacrylate alkyl ester to siloxane dianhydride compound is (1.9-2.1):

1.

6. The flexible water-based photocurable resin according to claim 5, characterized in that: The preparation method of the methacrylic acid alkyl ester comprises: adding glycidyl methacrylate, alkyl acid, catalyst and polymerization inhibitor into 1,4-dioxane, heating to 90-100° C., stirring and condensing reflux reaction for 4-8 hours, removing low boiling matters by vacuum distillation, adding water and dichloromethane, shaking and layering, extracting and separating, drying the organic phase to remove water, vacuum distillation, washing with petroleum ether and drying to obtain the methacrylic acid alkyl ester.

7. The flexible water-based photocurable resin according to claim 6, characterized in that: The molar ratio of the alkyl acid is glycidyl methacrylate, alkyl acid, catalyst and inhibitor is 1: (1-1.1): (0.0038-0.0045): (0.005-0.006).

8. The flexible water-based photocurable resin according to claim 7, characterized in that: The alkyl acid is decanoic acid, undecanoic acid, dodecanoic acid, tridecanoic acid or tetradecanoic acid; the catalyst is tetrabutylammonium bromide or triphenylphosphine; and the inhibitor is 4-methoxyphenol.

9. The flexible water-based photocurable resin according to claim 5, characterized in that: The preparation method of the siloxane dianhydride compound comprises: adding 1,3-bis(3-hydroxypropyl)-1,1,3,3-tetramethyldisiloxane, triethylamine and trimellitic anhydride chloride in a molar ratio of 1:(2-2.2):(2-2.2) to dichloromethane under an ice bath, then reacting at room temperature for 5-8 hours, distilling under reduced pressure, washing with water, drying and recrystallizing in ethyl acetate to obtain the siloxane dianhydride compound.

10. A method for preparing a flexible water-based photocurable resin according to any one of claims 1 to 9, characterized in that: The preparation method comprises adding waterborne polyurethane acrylate, active diluent, flexible waterborne siloxane crosslinking monomer, defoamer, emulsifier and neutralizer into water, stirring and mixing, and then adding photoinitiator to obtain flexible waterborne photocurable resin.