Polyacetal resin and preparation method thereof
The use of perchloric acid or perchlorate hydrate initiators in polyacetal resin production addresses the issues of high formaldehyde release and low mechanical strength, resulting in a resin with low emission and high strength, suitable for various applications.
Patent Information
- Application Number
- CN202411193966.1
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
Existing polyacetal resins suffer from high formaldehyde release rates and low mechanical strength due to the use of boron trifluoride and heteropolyacid catalysts, which have low catalytic activity, residual catalytic centers, and reactivity with impurities.
A polyacetal resin prepared using perchloric acid, perchlorate, or perchlorate hydrate as initiators, combined with specific comonomers, antioxidants, and controlled reaction conditions, to achieve low formaldehyde emission and high mechanical strength.
The resulting polyacetal resin exhibits formaldehyde emission below 25 ppm, tensile strength above 62 MPa, and bending strength above 2550 MPa, with improved process yield and stability.
Smart Images

Figure CN119081031A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a polyacetal resin and a preparation method thereof, and belongs to the field of chemical industry. Background Art
[0002] Polyacetal resin not only has excellent fatigue resistance, rigidity, self-lubrication, wear resistance, and corrosion resistance, but also has low water absorption. It is widely used in electronics, automobiles, daily necessities, precision instruments, agricultural equipment and other fields.
[0003] At present, boron trifluoride catalysts or heteropolyacid catalysts are often used as initiators to prepare polyacetal resins. Among them, boron trifluoride catalysts have low catalytic activity, are used in large quantities, and have a large amount of residues in the polymer product. Even after inactivation, there are still many catalytic active centers remaining. The obtained polyacetal resin is easy to cause molecular chain depolymerization to produce free formaldehyde under conditions such as light, heat, oxygen, and acid during use, and has the defect of high formaldehyde release; heteropolyacid catalysts are easy to react with impurities such as water, alcohol, and acid in the reaction raw materials and become inactivated. Therefore, the polyacetal resin prepared using heteropolyacid catalysts has the defect of low mechanical strength.
[0004] Therefore, developing a polyacetal resin with both low formaldehyde emission rate and high mechanical strength has become the current research direction. Summary of the invention
[0005] The invention provides a polyacetal resin, which has the characteristics of low formaldehyde release rate and high mechanical strength.
[0006] The invention also provides a method for preparing the polyacetal resin, which has the characteristic of high product yield.
[0007] The invention provides a polyacetal resin, wherein the formaldehyde emission of the polyacetal resin is not higher than 25 ppm, the tensile strength is not lower than 62 MPa, the bending strength is not lower than 2550 MPa, and the simply supported beam impact strength at 23°C is not lower than 6.5 kj / m2.
[0008] The polyacetal resin as described above, wherein the polyacetal resin is prepared by a preparation method comprising the following steps:
[0009] causing a mixed system including a main monomer, a comonomer, an initiator, a chain transfer agent, and an antioxidant to undergo a polymerization reaction to obtain a polyacetal resin;
[0010] The main monomer is formaldehyde or polyoxymethylene with a degree of polymerization not exceeding 10;
[0011] The comonomer is an epoxy compound;
[0012] The initiator is at least one of perchloric acid, perchlorate, and perchlorate hydrate.
[0013] The present invention also provides a method for preparing a polyacetal resin, by which any of the above-mentioned polyacetal resins can be prepared, comprising the following steps:
[0014] causing a mixed system including a main monomer, a comonomer, an initiator, a chain transfer agent, and an antioxidant to undergo a polymerization reaction to obtain a polyacetal resin;
[0015] The main monomer is formaldehyde or polyoxymethylene with a degree of polymerization not exceeding 10;
[0016] The comonomer is at least one of an epoxy compound and a cyclic acetal;
[0017] The initiator is one or more of perchloric acid, perchlorate, and perchlorate hydrate.
[0018] In the method for preparing the polyacetal resin as described above, the mass of the initiator is 1-60 ppm of the mass of the main monomer.
[0019] The method for preparing the polyacetal resin as described above, wherein the main monomer is trioxymethylene; and / or,
[0020] The comonomer is at least one of ethylene oxide, 1,3-dioxolane, 1,4-dioxane, 1,3-dioxepane, ethylene glycol formal, diethylene glycol formal, propylene glycol formal, and 1,4-butanediol formal, and the mass of the comonomer is 1-10wt% of the mass of the main monomer; and / or,
[0021] The chain transfer agent is at least one of methylal, acetal and butyral, and the mass of the chain transfer agent is 50-1500ppm of the mass of the main monomer; and / or,
[0022] The antioxidant is at least one of antioxidant 168, antioxidant 245, antioxidant 264, antioxidant 330, antioxidant 1010, antioxidant 1024, antioxidant 1076 and antioxidant 2246, and the mass of the antioxidant is 50-1500ppm of the mass of the main monomer.
[0023] The preparation method of the polyacetal resin as described above, wherein the mixed system further comprises a diluent, the diluent is used to dissolve the initiator, the diluent is at least one of 1,3-dioxolane, 1,4-dioxane, toluene, and tetrahydrofuran, and the mass of the diluent is 0.05-5wt% of the mass of the main monomer.
[0024] The method for preparing the polyacetal resin as described above, wherein the reaction temperature of the polymerization reaction is 40-150°C.
[0025] The method for preparing the polyacetal resin as described above further comprises mixing the product obtained by the polymerization reaction with a deactivator and a release agent, and then sequentially performing melt extrusion treatment, pulverization treatment, and drying treatment to obtain the polyacetal resin.
[0026] The method for preparing the polyacetal resin as described above, wherein the inactivator is at least one of triethylamine, triethanolamine, melamine and dimethylformamide, and the mass of the inactivator is 0.01-5wt% of the mass of the product; and / or,
[0027] The release agent is at least one of calcium stearate, magnesium stearate, zinc stearate, magnesium oxide, and ethylene bisstearamide, and the mass of the release agent is 0.01-5wt% of the mass of the product.
[0028] The method for preparing polyacetal resin as described above, wherein the particle size of the particles obtained by the pulverization process is 0.1-10 mm.
[0029] The polyacetal resin provided by the invention has low formaldehyde emission and high mechanical strength. BRIEF DESCRIPTION OF THE DRAWINGS
[0030] Figure 1 This is a flow chart of the preparation method used in Example 1. DETAILED DESCRIPTION
[0031] In order to enable those skilled in the art to better understand the scheme of the present invention, the present invention is further described in detail below. The specific implementation methods listed below are only for describing the principles and features of the present invention. The examples are only used to explain the present invention and are not intended to limit the scope of the present invention. Based on the embodiments of the present invention, all other implementation methods obtained by ordinary technicians in the field without creative work are within the scope of protection of the present invention.
[0032] The first aspect of the present invention provides a polyacetal resin, the formaldehyde emission of the polyacetal resin is not higher than 25ppm, the tensile strength is not lower than 62MPa, the flexural strength is not lower than 2550MPa, and the 23°C simply supported beam impact strength is not lower than 6.5kj / ㎡.
[0033] The polyacetal resin provided by the present invention has low formaldehyde emission and high mechanical strength. Therefore, the polyacetal resin provided by the present invention is friendly to the environment and the health of users.
[0034] In one embodiment, the polyacetal resin provided by the present invention can be prepared by the following steps:
[0035] causing a mixed system including a main monomer, a comonomer, an initiator, a chain transfer agent, and an antioxidant to undergo a polymerization reaction to obtain a polyacetal resin;
[0036] The main monomer is formaldehyde or polyoxymethylene with a degree of polymerization not exceeding 10;
[0037] The comonomer is at least one of an epoxy compound and a cyclic acetal;
[0038] The initiator is one or more of perchloric acid, perchlorate, and perchlorate hydrate.
[0039] The main monomer refers to a monomer molecule that can be repeatedly combined to form a polymer in a polymerization reaction. In the polymerization process, the main monomers are connected by covalent bonds to form a high molecular weight polymer. The present invention uses formaldehyde or polyoxymethylene with a degree of polymerization of no more than 10 as the main monomer, and the specific degree of polymerization within the above range is not limited, and the selected main monomer can meet the requirements of producing polyacetal resin.
[0040] The comonomer refers to a monomer that participates in the polymerization reaction simultaneously with the main monomer. The present invention uses at least one of epoxy compounds and cyclic acetals as the comonomer. Among them, the comonomer can be selected from epoxy compounds only, cyclic acetals only, or epoxy compounds and cyclic acetals at the same time. The present invention does not limit the specific selection of the comonomer, and the selected comonomer can be selected to react with the main monomer to obtain a polyacetal resin.
[0041] The initiator can start or promote the polymerization reaction of monomer molecules to form a high molecular weight polymer. The present invention uses one or more of perchloric acid, perchlorate, and perchlorate hydrate as an initiator, wherein the perchlorate is one or more of sodium perchlorate, potassium perchlorate, magnesium perchlorate, calcium perchlorate, iron perchlorate, copper perchlorate, zinc perchlorate, and aluminum perchlorate. The perchlorate hydrate is one or more of sodium perchlorate hydrate, potassium perchlorate hydrate, magnesium perchlorate hydrate, calcium perchlorate hydrate, iron perchlorate hydrate, copper perchlorate hydrate, zinc perchlorate, and aluminum perchlorate hydrate. The present invention does not limit the specific selection of the initiator within the above range, and the selected initiator satisfies the requirement of being able to undergo polymerization reaction with the main monomer to obtain the polyacetal resin.
[0042] Chain transfer agents can affect the growth process of polymer chains and transfer the active center on a polymer chain to another molecule. Therefore, the introduction of chain transfer agents can regulate the molecular weight distribution and structure of polymers. The present invention does not specifically limit the selection of chain transfer agents, as long as the requirements for producing polyacetal resins are met. In one embodiment, the chain transfer agent is at least one of acetal compounds.
[0043] The antioxidant can prevent the polymer product from being depolymerized under high temperature conditions during subsequent processing and producing formaldehyde. The present invention does not specifically limit the selection of the antioxidant, and the antioxidant can be selected from the commonly used antioxidants in the art. In one embodiment, the antioxidant is a hindered phenol antioxidant.
[0044] The inventors have found that when at least one of perchloric acid, perchlorate, and perchlorate hydrate is used as an initiator, the obtained polyacetal resin has high mechanical strength and low formaldehyde release rate. The inventors speculate that the reason may be that, firstly, perchloric acid, perchlorate, and perchlorate hydrate are highly active initiators, which can make the main monomer and the comonomer undergo polymerization reaction to generate a polyacetal resin with high mechanical strength; secondly, since perchloric acid, perchlorate, and perchlorate hydrate initiators have high activity, the amount used is small, and the residual amount in the polyacetal resin is also small. Therefore, the polyacetal resin releases less formaldehyde when the molecular chain is depolymerized under the conditions of light, heat, oxygen, acid, etc.
[0045] The second aspect of the present invention provides a method for preparing a polyacetal resin, which can be used to prepare any of the above-mentioned polyacetal resins. The preparation method comprises the following steps:
[0046] causing a mixed system including a main monomer, a comonomer, an initiator, a chain transfer agent, and an antioxidant to undergo a polymerization reaction to obtain a polyacetal resin;
[0047] The main monomer is formaldehyde or polyoxymethylene with a degree of polymerization not exceeding 10;
[0048] The comonomer is an epoxy compound;
[0049] The initiator is at least one of perchloric acid, perchlorate, and perchlorate hydrate.
[0050] The selection of main monomer, comonomer, initiator, chain transfer agent and antioxidant can refer to the above content.
[0051] The inventors have found that when at least one of perchloric acid, perchlorate, and perchlorate hydrate is used as an initiator, the obtained polyacetal resin has high mechanical strength and low formaldehyde release rate. The inventors speculate that the reason may be that, firstly, perchloric acid, perchlorate, and perchlorate hydrate are highly active initiators, which can make the main monomer and the comonomer undergo polymerization reaction to generate a polyacetal resin with high mechanical strength; secondly, since perchloric acid, perchlorate, and perchlorate hydrate initiators have high activity, the amount used is small, and the residual amount in the polyacetal resin is small. Therefore, the formaldehyde release of the polyacetal resin due to molecular chain decomposition under the conditions of light, heat, oxygen, acid, etc. is also small.
[0052] In addition, the inventors also found that since at least one of perchloric acid, perchlorate, and perchlorate hydrate is insensitive to impurities such as water, alcohol, and acid in the raw materials participating in the polymerization reaction when used as an initiator, the initiator is inactivated. Therefore, when the above substances are used as initiators, the yield rate of the preparation process is high, and polyacetal resin with stable quality can be produced.
[0053] The preparation method of the polyacetal resin provided by the present invention uses at least one of perchloric acid, perchlorate and perchlorate hydrate as an initiator, which can not only produce the polyacetal resin with low formaldehyde release rate and high mechanical strength, but also enable the production process of the polyacetal resin to have the advantage of high yield rate.
[0054] In one embodiment, the mass of the initiator is 1-60 ppm of the mass of the main monomer. Controlling the amount of the initiator added within the above range can not only improve the reaction efficiency of the polymerization reaction, but also reduce the risk of explosion and heat release due to excessive initiator addition, which is difficult to remove in time, and the hardness of the polymer product increases sharply, causing the reactor to be blocked.
[0055] Further, in one embodiment, the main monomer may be trioxymethylene, and the comonomer may be at least one of ethylene oxide, 1,3-dioxolane, 1,4-dioxane, 1,3-dioxepane, ethylene glycol formal, diethylene glycol formal, propylene glycol formal, and 1,4-butanediol formal, and the mass of the comonomer is 1-10wt% of the mass of the main monomer. Controlling the mass ratio of the comonomer to the main monomer within the above range can make the obtained polyacetal resin have a higher mechanical strength and a lower formaldehyde emission.
[0056] In one embodiment, the chain transfer agent is at least one of methylal, acetal, and butyral, and the mass of the chain transfer agent is 50-1500ppm of the mass of the main monomer. Controlling the amount of the chain transfer agent to be added within the above range can make the obtained polyacetal resin have suitable fluidity under the premise of high mechanical strength and the advantage of not being easy to block the reactor pipeline.
[0057] Further, in one embodiment, the antioxidant is at least one of antioxidant 168, antioxidant 245, antioxidant 264, antioxidant 330, antioxidant 1010, antioxidant 1024, antioxidant 1076 and antioxidant 2246, and the mass of the antioxidant is 50-1500 ppm of the mass of the main monomer. Controlling the amount of the antioxidant to be added within the above range can make the obtained polyacetal resin more thermally stable and have a lower formaldehyde emission.
[0058] In one embodiment, the mixed system further includes a diluent, which is used to dissolve the initiator, and the diluent is at least one of 1,3-dioxolane, 1,4-dioxane, toluene, and tetrahydrofuran, and the mass of the diluent is 0.05-5wt% of the mass of the main monomer. Using the above amount of diluent to dissolve the initiator can make the initiator evenly distributed in the raw material system, which helps to improve the efficiency of the polymerization reaction, so that the preparation method of the polyacetal resin provided by the present invention is more efficient.
[0059] Furthermore, in one embodiment, the reaction temperature of the polymerization reaction can be controlled to be 40-150° C. Controlling the reaction temperature of the polymerization reaction within the above range can make the polymerization reaction more efficient while having lower safety risks.
[0060] In one embodiment, the method for preparing the polyacetal resin provided by the present invention further comprises mixing the product obtained by the polymerization reaction with a deactivator and a release agent, and then sequentially performing melt extrusion treatment, pulverization treatment, and drying treatment to obtain the polyacetal resin.
[0061] The inactivator can react chemically with the residual initiator in the product obtained by the polymerization reaction to render the initiator ineffective, so that the obtained polyacetal resin is not easy to decompose and produce free formaldehyde under the action of the initiator, and thus has a lower formaldehyde release. The preparation method provided by the present invention does not specifically limit the selection of the inactivator, and it only needs to meet the requirement of being able to react with the initiator to render the initiator ineffective. The preparation method provided by the present invention also does not specifically limit the dosage of the inactivator, and it only needs to remove the residual inactivator in the polymerization product.
[0062] The addition of a release agent helps the molding of polyacetal resin, and can make the polyacetal resin product have good processability. Specifically, the use of a release agent makes it difficult for the polyacetal resin product to remain on the surface of the injection mold, and has a low degree of influence on the shape of the injection molded product. The preparation method provided by the present invention does not specifically limit the selection of a release agent, and a release agent commonly used in the art can be selected. The preparation method provided by the present invention also does not specifically limit the amount of the release agent added, and it only needs to meet the requirement of improving the processability of the polyacetal resin material.
[0063] During the melt extrusion process, the polymer product is heated to a flowable state, which facilitates granulation and removes the unstable terminal groups and free formaldehyde remaining in the polymer product, so that the obtained polyacetal resin has a lower formaldehyde release. In one embodiment, the processing temperature of the melt extrusion process is 90-180° C. Controlling the processing temperature of the melt extrusion process to the above range can not only remove the unstable terminal groups and free formaldehyde remaining in the polymer product, but also avoid the free formaldehyde generated by the polymer product due to high temperature decomposition.
[0064] During the pulverization process, the polymer product that has undergone melt extrusion treatment is pulverized into granules, which is convenient for packaging and subsequent processing; and the drying process can remove the residual formaldehyde and moisture in the granular polyacetal resin obtained by the pulverization process, so that the obtained polyacetal resin has a higher purity.
[0065] It is understandable that, in order to facilitate the melt extrusion process, in one embodiment, before performing the melt base treatment, the polymer product is also pre-crushed to make it into particles with a particle size of 0.5-5.0 mm, and the above particles are used for melt extrusion processing.
[0066] In one embodiment, the inactivator is at least one of triethylamine, triethanolamine, melamine and dimethylformamide, and the mass of the inactivator is 0.01-5wt% of the mass of the product. Controlling the amount of the inactivator to be added within the above range can make the obtained polyacetal resin product have higher purity under the premise of effectively removing the initiator.
[0067] Further, in one embodiment, the release agent is at least one of calcium stearate, magnesium stearate, zinc stearate, magnesium oxide, and ethylene bis stearamide, and the mass of the release agent is 0.01-5wt% of the mass of the product. Controlling the amount of the release agent to be added within the above range can make the obtained polyacetal resin have better processability and higher purity.
[0068] Furthermore, controlling the particle size of the particles obtained by the pulverization process to 0.1-10 mm is beneficial to the drying, packaging and reprocessing of the product. In one embodiment, the pulverization process is performed by underwater pelletizing.
[0069] In one embodiment, the drying temperature is controlled to be 100-250° C. and the drying time is 2 hours, which can more thoroughly remove the residual free formaldehyde and moisture in the polyacetal resin and make it have a higher purity. Specifically, during the drying process, air or nitrogen with the above temperature range can be used for purging.
[0070] The preparation method of the polyacetal resin provided by the present invention will be described in detail below with reference to specific embodiments.
[0071] Example 1
[0072] The present invention provides a method for preparing a polyacetal resin, such as Figure 1 As shown, the following steps are included:
[0073] 1) dissolving 0.0012 g of a perchloric acid initiator in 2 g of a 1,4-dioxane solvent, and adding the mixture into a polymerization reactor together with 100 g of trioxymethylene, 3 g of a 1,4-dioxane comonomer, 0.05 g of a methylal chain transfer agent, and 0.04 g of an antioxidant 1076, to carry out a polymerization reaction at a reaction temperature of 90° C. and a reaction pressure of normal pressure to obtain a polymerization product;
[0074] 2) The above polymer product is crushed into particles with an average diameter of 2.5 mm by a crusher, 0.05 g of triethanolamine inactivator and 1 g of magnesium oxide release agent are added and mixed evenly, and melt extrusion treatment is performed in a container. The treatment temperature of the melt extrusion treatment is 120° C., and the melt extrusion treatment pressure is -0.09 MPaG to obtain a melt extrusion treatment product;
[0075] 3) The melt extrusion product was cooled, molded and cut into particles with an average diameter of 5 mm, and dried with hot air at 140° C. for 3 h to obtain a polyacetal resin sample A1.
[0076] Example 2
[0077] 1) 0.002 g of zinc perchlorate initiator was dissolved in 1 g of tetrahydrofuran solvent, and added into a polymerization reactor together with 100 g of trioxymethylene, 5 g of 1,3-dioxepane comonomer, 0.04 g of acetal chain transfer agent, and 0.05 g of antioxidant 245. A polymerization reaction was carried out at a reaction temperature of 140° C. and a reaction pressure of normal pressure to obtain a polymerization product;
[0078] 2) crushing the above-mentioned polymer product into particles with an average diameter of 5 mm by a crusher, adding 0.02 g of melamine inactivator and 2 g of zinc stearate release agent and mixing them evenly, and performing melt extrusion treatment in a container, the treatment temperature of the melt extrusion treatment is 150° C., and the treatment pressure is -0.08 MPaG, to obtain a melt extrusion treatment product;
[0079] 3) The melt extrusion product was cooled, molded and cut into particles with an average diameter of 3 mm, and dried with hot air at 160° C. for 2 h to obtain a polyacetal resin sample A2.
[0080] Example 3
[0081] This embodiment is substantially the same as embodiment 1, except that in step 1), the mass of perchloric acid is 0.0005 g.
[0082] A polyacetal resin sample A3 was obtained.
[0083] Example 4
[0084] This embodiment is substantially the same as embodiment 1, except that in step 1), the mass of the 1,4-dioxane comonomer is 8 g.
[0085] A polyacetal resin sample A4 was obtained.
[0086] Example 5
[0087] This embodiment is substantially the same as embodiment 1, except that in step 1), the mass of the methylal chain transfer agent is 0.01 g.
[0088] A polyacetal resin sample A5 was obtained.
[0089] Example 6
[0090] This embodiment is basically the same as embodiment 1, except that in step 1), the reaction temperature of the polymerization reaction is 120°C.
[0091] A polyacetal resin sample A6 was obtained.
[0092] Example 7
[0093] This embodiment is substantially the same as embodiment 1, except that, in step 2), the mass of the triethanolamine inactivator is 0.02 g.
[0094] A polyacetal resin sample A7 was obtained.
[0095] Example 8
[0096] This embodiment is substantially the same as the embodiment 1, except that 0.0017 g of potassium perchlorate dissolved in 2 g of 1,4-dioxane is used as an initiator to obtain a polyacetal resin sample A8.
[0097] Example 9
[0098] This embodiment is substantially the same as embodiment 1, except that the same mass of ethylene oxide as in embodiment 1 is used as a comonomer.
[0099] A polyacetal resin sample A9 was obtained.
[0100] Example 10
[0101] This embodiment is substantially the same as embodiment 1, except that in step 1), the mass of the perchloric acid initiator is 0.001 g.
[0102] A polyacetal resin sample A10 was prepared.
[0103] Embodiment 11
[0104] This embodiment is substantially the same as embodiment 1, except that in step 1), the mass of the dioxane comonomer is 20 g.
[0105] A polyacetal resin sample A11 was obtained.
[0106] Example 12
[0107] This embodiment is substantially the same as embodiment 1, except that, in step 2), the mass of the triethanolamine inactivator is 0.005 g.
[0108] A polyacetal resin sample A12 was obtained.
[0109] Comparative Example 1
[0110] This comparative example is substantially the same as Example 1, except that, in step 1), 0.05 g of boron trifluoride etherate is dissolved in 5 g of cyclohexane as an initiator.
[0111] Sample B1 was prepared.
[0112] Comparative Example 2
[0113] This comparative example is basically the same as Example 1, except that in step 1), 0.0005 g of phosphotungstic acid is dissolved in 1 g of ethyl acetate as an initiator.
[0114] Sample B2 was prepared.
[0115] Test example
[0116] 1. The yield rates of the samples obtained in the above embodiments and comparative examples were measured, and the results are shown in Table 1.
[0117] The yield rate is determined as follows:
[0118] According to the above embodiments and comparative examples, the corresponding polyacetal resin products were prepared, and the tensile strength was measured according to ISO527 standard, and the simply supported beam impact strength was measured according to ISO179 / 1eA standard. Ten groups of samples were prepared for testing in each embodiment and comparative example, and the samples with a tensile strength of not less than 55MPa and a simply supported beam impact strength of not less than 5.5kj / ㎡ at 23°C were considered qualified, otherwise they were considered unqualified. The number of qualified samples ÷ 10 × 100% is the yield rate of the embodiment or comparative example.
[0119] Table 1 Yield Rate Record
[0120]
[0121]
[0122] It can be seen from Table 1 that compared with the samples prepared in the comparative example, the samples prepared in each embodiment have a higher yield rate.
[0123] 2. Perform the following tests on samples A1-A12, B1, and B2:
[0124] 1) Determine the tensile strength of each of the above samples according to ISO527 standard;
[0125] 2) Determine the bending strength of each of the above samples according to ISO178 standard;
[0126] 3) Determine the simply supported beam impact strength of the above samples according to ISO179 / 1eA standard;
[0127] 4) Determine the formaldehyde emission of each of the above samples according to VDA275 standard;
[0128] The above measurement data are shown in Table 2.
[0129] Table 2 Sample characteristics record table
[0130]
[0131] It can be seen from Table 2 that compared with the samples prepared in the comparative example, the samples prepared in the embodiments have higher mechanical strength and lower formaldehyde emission, which indicates that the polyacetal resin provided by the present invention has the characteristics of lower formaldehyde emission rate and higher mechanical strength.
[0132] Furthermore, the mechanical strength of A11 and A12 is lower than that of A1-A10, and the formaldehyde emission is higher than that of A1-A10, which may be due to the excessively high quality of the copolymer monomer in the preparation process of A11 and the excessively low quality of the inactivator in the preparation process of A12.
[0133] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A polyacetal resin, characterized in that The formaldehyde emission of the polyacetal resin is not higher than 25 ppm, the tensile strength is not lower than 62 MPa, the flexural strength is not lower than 2550 MPa, and the 23° C. simply supported beam impact strength is not lower than 6.5 kj / m2.
2. The polyacetal resin according to claim 1, characterized in that Prepared by a preparation method comprising the following steps: causing a mixed system including a main monomer, a comonomer, an initiator, a chain transfer agent, and an antioxidant to undergo a polymerization reaction to obtain a polyacetal resin; The main monomer is formaldehyde or polyoxymethylene with a degree of polymerization not exceeding 10; The comonomer is at least one of an epoxy compound and a cyclic acetal; The initiator is at least one of perchloric acid, perchlorate, and perchlorate hydrate.
3. A method for preparing a polyacetal resin, characterized in that: The following steps are involved: causing a mixed system including a main monomer, a comonomer, an initiator, a chain transfer agent, and an antioxidant to undergo a polymerization reaction to obtain a polyacetal resin; The main monomer is formaldehyde or polyoxymethylene with a degree of polymerization not exceeding 10; The comonomer is an epoxy compound; The initiator is at least one of perchloric acid, perchlorate, and perchlorate hydrate.
4. The preparation method according to claim 3, characterized in that: The mass of the initiator is 1-60 ppm of the mass of the main monomer.
5. The preparation method according to claim 3 or 4, characterized in that: The main monomer is trioxymethylene; and / or, The comonomer is at least one of ethylene oxide, 1,3-dioxolane, 1,4-dioxane, 1,3-dioxepane, ethylene glycol formal, diethylene glycol formal, propylene glycol formal, and 1,4-butanediol formal, and the mass of the comonomer is 1-10wt% of the mass of the main monomer; and / or, The chain transfer agent is at least one of methylal, acetal and butyral, and the mass of the chain transfer agent is 50-1500ppm of the mass of the main monomer; and / or, The antioxidant is at least one of antioxidant 168, antioxidant 245, antioxidant 264, antioxidant 330, antioxidant 1010, antioxidant 1024, antioxidant 1076 and antioxidant 2246, and the mass of the antioxidant is 50-1500ppm of the mass of the main monomer.
6. The preparation method according to any one of claims 3 to 5, characterized in that: The mixed system further includes a diluent, which is used to dissolve the initiator. The diluent is at least one of 1,3-dioxolane, 1,4-dioxane, toluene and tetrahydrofuran, and the mass of the diluent is 0.05-5wt% of the mass of the main monomer.
7. The preparation method according to any one of claims 3 to 6, characterized in that: The reaction temperature of the polymerization reaction is 40-150°C.
8. The preparation method according to any one of claims 3 to 7, characterized in that: The method also includes mixing the product obtained by the polymerization reaction with an inactivator and a release agent, and then sequentially performing melt extrusion treatment, pulverization treatment, and drying treatment to obtain a polyacetal resin.
9. The preparation method according to claim 8, characterized in that: The inactivator is at least one of triethylamine, triethanolamine, melamine and dimethylformamide, and the mass of the inactivator is 0.01-5wt% of the mass of the product; and / or, The release agent is at least one of calcium stearate, magnesium stearate, zinc stearate, magnesium oxide, and ethylene bisstearamide, and the mass of the release agent is 0.01-5wt% of the mass of the product.
10. The preparation method according to claim 8 or 9, characterized in that: The particle size of the particles obtained by the pulverization process is 0.1-10 mm.