Biodegradable polyester copolymer as well as preparation method and application thereof
By optimizing the esterification and copolymerization of aromatic and aliphatic dicarboxylic acids with PLA, the biodegradable polyester copolymer achieves improved mechanical properties and biodegradability, overcoming compatibility challenges in existing blends.
Patent Information
- Application Number
- CN202310662661.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2023-06-06
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2043-06-06
AI Technical Summary
The poor compatibility between aliphatic-aromatic polyesters and PLA results in poor mechanical properties and stability of biodegradable plastic alloys, with existing methods failing to achieve efficient copolymerization and phase refinement.
A method involving controlled esterification and copolymerization of aromatic and aliphatic dicarboxylic acid compounds with polylactic acid, optimizing reaction conditions to achieve a biodegradable polyester copolymer with improved compatibility and mechanical properties.
The biodegradable polyester copolymer exhibits enhanced tensile strength, elongation at break, and biodegradability, with the PLA phase uniformly dispersed, addressing the compatibility issues of previous methods.
Smart Images

Figure BDA0004269672580000071 
Figure BDA0004269672580000081 
Figure BDA0004269672580000091
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of biodegradable plastics, in particular to a biodegradable polyester copolymer and a preparation method and application thereof. Background Art
[0002] Aliphatic-aromatic polyesters represented by PBAT (copolymer of butylene adipate and butylene terephthalate) have excellent biodegradability and are one of the most widely used biodegradable materials. Aliphatic-aromatic polyesters have the characteristics of both aliphatic polyesters and aromatic polyesters, with good ductility and elongation at break, but poor impact strength, especially at low temperatures.
[0003] Polylactic acid, referred to as PLA, also known as polyhydroxypropionic acid or polylactide, is a biodegradable polymer material formed by the polycondensation of lactic acid monomers. PLA has high strength, but poor toughness, lacks elasticity and flexibility, is hard and brittle, has low elongation at break; and the crystallization rate of PLA is too slow, and the processing performance is poor.
[0004] The blending of aliphatic-aromatic polyester and PLA can, on the one hand, produce biodegradable plastic alloys with high bio-based content; on the other hand, it can achieve complementary performance. PLA can improve the impact strength of aliphatic-aromatic polyester, while aliphatic-aromatic polyester can better improve the processing performance and elongation at break of PLA.
[0005] However, the solubility parameters of PLA and aliphatic-aromatic polyester are quite different, and the compatibility of the two is poor. Without the addition of a compatibilizer, the comprehensive performance of the PLA / aliphatic-aromatic polyester alloy is poor. After the compatibilizer is used to increase the volume, the blend morphology is still a phase separation structure, and it is difficult to ensure that the dispersed phase is fully refined. Prior art CN102702696A discloses a fully degradable biomaterial composed of PBAT and PLA, wherein PBAT accounts for 75-90wt.%, and the rest is PLA. This fully degradable biomaterial has the problem of compatibility between PLA and PBAT, and the performance and stability of the product cannot be guaranteed, and it is difficult to use it for a long time.
[0006] In order to solve the problem of poor compatibility between the above-mentioned aliphatic-aromatic polyester and PLA, the prior art CN104725620A discloses an unsaturated polylactic acid block copolymer and a preparation method thereof, comprising first preparing an unsaturated copolyester, and then reacting the unsaturated copolyester with lactide under the action of a catalyst to obtain an unsaturated polylactic acid block copolymer. However, the reaction conditions of lactide and unsaturated copolyester are harsh and poor in controllability, the obtained unsaturated polylactic acid block copolymer has low yield and poor efficiency, and the compatibility between PLA and aliphatic-aromatic polyester is still poor, resulting in insufficient mechanical properties of the unsaturated polylactic acid block copolymer. Summary of the invention
[0007] The purpose of the present invention is to overcome the defect of poor compatibility between aliphatic-aromatic polyester and PLA in the prior art and to provide a biodegradable polyester copolymer.
[0008] Another object of the present invention is to provide a method for preparing the above-mentioned biodegradable polyester copolymer.
[0009] Another object of the present invention is to provide applications of the biodegradable polyester copolymer.
[0010] To achieve the above object, the present invention adopts the following technical solution:
[0011] A method for preparing a biodegradable polyester copolymer comprises the following steps:
[0012] S1. An aromatic dicarboxylic acid compound, 1,4-butanediol and a catalyst are mixed to perform an esterification reaction to obtain an esterified product E1, wherein the terminal carboxyl content of the esterified product E1 is 50 to 450 mol / t;
[0013] S2. mixing an aliphatic dicarboxylic acid compound with 1,4-butanediol, and performing an esterification reaction to obtain an esterified product E2, wherein the terminal carboxyl content of the esterified product E2 is 500 to 5000 mol / t;
[0014] S3. The esterified product E1, the esterified product E2 and the polylactic acid are mixed, added to a copolymerization reaction device, and reacted at 200-250° C. and 1000-5000 Pa for 1.5-4 hours to obtain a biodegradable polyester copolymer.
[0015] Based on the total molar amount of the aromatic dicarboxylic acid compound and the aliphatic dicarboxylic acid compound, the aromatic dicarboxylic acid compound accounts for 38 to 52 mol%, and the aliphatic dicarboxylic acid compound accounts for 48 to 62 mol%;
[0016] The D-type content of the polylactic acid is 0.4-1.6%, and the melting point of the polylactic acid is 150-180°C.
[0017] The content of aromatic dicarboxylic acid compounds in aliphatic-aromatic polyesters directly affects the mechanical properties, thermodynamic properties, degradation properties and processing properties of aliphatic-aromatic polyesters. Based on the total molar amount of aromatic dicarboxylic acid compounds and aliphatic dicarboxylic acid compounds, when aromatic dicarboxylic acid compounds account for 38-52 mol%, the melting point of the corresponding aliphatic-aromatic polyester is 105-123°C.
[0018] The aromatic dicarboxylic acid compound in the present invention refers to a derivative of an aromatic dicarboxylic acid or its ester, or a mixture thereof; the aliphatic dicarboxylic acid compound refers to a derivative of an aliphatic dicarboxylic acid or its ester, or a mixture thereof.
[0019] Preferably, the aromatic dicarboxylic acid is at least one of terephthalic acid, dimethyl terephthalate, diethyl terephthalate, dibutyl terephthalate, dioctyl terephthalate, ethylene terephthalate, butylene terephthalate, isophthalic acid, dioctyl isophthalate, naphthalene dicarboxylic acid, and diphenyl dicarboxylic acid.
[0020] Preferably, the aliphatic dicarboxylic acid is at least one of succinic acid, adipic acid, suberic acid and sebacic acid.
[0021] In the preparation method of the biodegradable polyester copolymer of the present invention, an aromatic dicarboxylic acid compound and an aliphatic dicarboxylic acid compound are first subjected to esterification reaction with 1,4-butanediol to obtain two esters, and then the esters E1 and E2 are mixed with polylactic acid for copolymerization reaction. During the copolymerization reaction, the esters E1 and E2 react to obtain copolyester, and the polylactic acid also achieves good compatibility with the copolyester. The present invention reasonably controls the esterification reaction conditions and the copolymerization reaction conditions, so that the obtained biodegradable polyester copolymer has both the high strength of polylactic acid and the high toughness of aliphatic-aromatic polyester, and also has good biodegradability.
[0022] The method for detecting the terminal carboxyl content in the esterification product is in accordance with FZ / T 50012 2006 "Titration analysis method for determining the terminal carboxyl content in polyester": using a mixture of o-cresol and chloroform as solvent, the mass ratio of o-cresol to chloroform is 7:3, and using an automatic potentiometric titrator to test the terminal carboxyl value.
[0023] The terminal carboxyl content of the esterified product reflects the degree of esterification reaction. The lower the terminal carboxyl content, the more thorough the esterification reaction, and the lower the terminal carboxyl content, the lower the degree of esterification reaction. The inventors have found that controlling the terminal carboxyl content of the esterified product E1 to be relatively small, 50 to 450 mol / t, and controlling the terminal carboxyl content of the esterified product E2 to be relatively high, 500 to 5000 mol / t, is conducive to the copolymerization reaction in the subsequent step S3. When the terminal carboxyl content range is exceeded, the efficiency of the copolymerization reaction is poor, or the PLA phase in the biodegradable polyester copolymer is difficult to disperse well.
[0024] Preferably, in step S1, an aromatic dicarboxylic acid compound is mixed with a portion of 1,4-butanediol to obtain a mixture A; the remaining 1,4-butanediol is mixed with a catalyst to obtain a mixture B, and then the mixture A and the mixture B are respectively added to an esterification reaction device for reaction.
[0025] The viscosity of the catalyst is high, and adding the catalyst directly will easily cause it to stick to the wall, which will affect the catalytic effect. By dissolving the catalyst in 1,4-butanediol and then adding it, the catalytic effect of the catalyst can be improved.
[0026] Preferably, the terminal carboxyl content of the esterified product E1 is 100 to 400 mol / t.
[0027] Preferably, the terminal carboxyl content of the esterified product E2 is 2000-3000 mol / t.
[0028] When the terminal carboxyl content of the esterified product E1 and the esterified product E2 is within the above preferred range, the mechanical properties of the obtained biodegradable polyester copolymer are better.
[0029] Preferably, in step S1, the esterification reaction is carried out at 200-250°C and 30-110 KPa for 1.5-3.5 hours.
[0030] Preferably, in step S2, the esterification reaction is carried out at 150-200° C. and 30-110 KPa for 2-4 hours.
[0031] Preferably, the catalyst is a titanate catalyst.
[0032] Optionally, the titanate catalyst is at least one of n-butyl titanate, n-ethyl titanate, tetraisopropyl titanate, a titanocene catalyst, and a chelated titanate catalyst.
[0033] Preferably, the intrinsic viscosity of the polylactic acid is 0.2 to 1.2 dL / g, preferably 0.2 to 1.0 dL / g.
[0034] The testing method for the intrinsic viscosity of polylactic acid is GB / T 10247-2008, the solvent used includes chloroform or dichloromethane, and the testing temperature is 25°C.
[0035] The viscosity of polylactic acid should not be too high. When the viscosity is too high, polylactic acid is not easy to copolymerize with ester E1 and ester E2, or the PLA phase in the biodegradable polyester copolymer is still difficult to be well compatible. The inventors found that when the viscosity of PLA is 0.2-1.2 dL / g, the copolymerization reaction can be carried out efficiently, and the PLA phase in the biodegradable polyester copolymer is well dispersed.
[0036] The D-type content of polylactic acid PLA can be detected by the following method: use a catalyst to hydrolyze polylactic acid in methanol so that all lactic acid monomers in the molecule are converted into methyl lactate, and then analyze it by gas chromatography. The peak area ratio of D-methyl lactate to L-methyl lactate is the D-type content in polylactic acid.
[0037] The D-type content of polylactic acid can be specifically detected according to the following steps: (1) Weigh 100±10 mg of polylactic acid sample and place it in a 25 mL pressurized container; (2) Add 10 mL of methanol and 1 drop of dilute sulfuric acid with a concentration of 20 wt.%; (3) Seal the pressurized container and place it in a 150°C thermostat for 4 hours; (4) Take out the pressurized container and open the lid after the container cools to room temperature; (5) After the sample solution is filtered through a membrane filter (pore size 0.22 or 0.45 μm), transfer it to a special injection vial for gas chromatography and operate according to the equipment manufacturer's instructions; (6) Calculate the D-type content based on the peak area ratio.
[0038] Preferably, based on the total amount of the ester E1, the ester E2 and the polylactic acid, the weight of the polylactic acid accounts for 8 to 41 wt.%.
[0039] Preferably, in step S3, the viscosity number (intrinsic viscosity) of the biodegradable polyester copolymer is 1.2-1.8 dL / g.
[0040] The present invention also protects a biodegradable polyester copolymer prepared by the above preparation method.
[0041] The number average molecular weight Mn of the biodegradable polyester copolymer is 50,000-120,000, preferably 62,000-113,000.
[0042] The number average molecular weight Mn of the biodegradable polyester copolymer can be measured by gel permeation chromatography (GPC). It can be determined by using a set of two columns in series (particle sizes of 5 μm and 3 μm, with mixed porosity), a refractive index detector, chloroform as eluent (flow rate 0.5 ml / min) and polystyrene as reference standard while maintaining the chromatography system at 40°C.
[0043] The melting point of the biodegradable polyester copolymer can be tested by differential scanning calorimetry (DSC). Specifically, 5-10 mg of the sample is weighed and placed in a crucible used for DSC testing. The temperature is raised in the range of 20 to 200°C at a rate of 10K / min. Two cycles of testing are performed. The peak value corresponding to the melting peak on the second heating curve is the melting point of the sample.
[0044] For the physical mixture of aliphatic-aromatic polyester and polylactic acid, due to the poor compatibility between the two, the melting points of aliphatic-aromatic polyester and polylactic acid will be shown separately in the second heating curve of DSC. For the biodegradable polyester copolymer composed of aliphatic-aromatic polyester and polylactic acid described in the present invention, during the synthesis process, due to the bonding reaction between chemical bonds, the compatibility of aliphatic-aromatic polyester and polylactic acid is improved. For a partially compatible system, two melting point peaks will appear in the second heating curve of DSC; for a completely compatible system, only one melting point peak will appear, and the corresponding melting point value is between the melting point peaks of the individual aliphatic-aromatic polyester and polylactic acid. Therefore, the compatibility of aliphatic-aromatic polyester and polylactic acid in the biodegradable polyester copolymer can be judged by the change in the melting point of the sample.
[0045] The difference η between the melting point corresponding to the polylactic acid component in the biodegradable polyester copolymer of the present invention and the theoretical melting point of the biodegradable polyester copolymer is ≤22°C, preferably ≤15°C.
[0046] The theoretical melting point of the biodegradable polyester copolymer of the present invention refers to the melting point of the corresponding sample when the aliphatic-aromatic polyester is completely compatible with polylactic acid. The theoretical melting point can be calculated by the formula shown in formula (I):
[0047] M p(理论) =M p1 *W1+M p2 *W2 Formula (I)
[0048] in,
[0049] M p(理论) , the melting point of the biodegradable polyester copolymer when the aliphatic-aromatic polyester is fully compatible with polylactic acid;
[0050] M p1 , melting points of individual aliphatic-aromatic polyesters;
[0051] M P2 , melting point of polylactic acid alone;
[0052] W1, weight percentage of aliphatic-aromatic polyester in the biodegradable polyester copolymer;
[0053] W2, weight percentage of polylactic acid in the biodegradable polyester copolymer.
[0054] The difference η between the melting point corresponding to the polylactic acid component in the biodegradable polyester copolymer and the theoretical melting point of the biodegradable polyester copolymer can be calculated by the formula shown in formula (II):
[0055] η= M P2 -M p(理论) Formula (II)
[0056] The biodegradable polyester copolymer prepared by the preparation method has good tensile strength and elongation at break, and good biodegradability.
[0057] The present invention also protects the use of the biodegradable polyester copolymer in preparing disposable film bags.
[0058] Compared with the prior art, the present invention has the following beneficial effects:
[0059] The present invention provides a biodegradable polyester copolymer, comprising a PBAT-type polyester phase and a PLA phase, and the two phases have good compatibility. The biodegradable polyester copolymer has excellent tensile strength and elongation at break, and has good biodegradability. DETAILED DESCRIPTION
[0060] In order to better illustrate the purpose, technical solutions and advantages of the present invention, the present invention will be further described below in conjunction with specific embodiments, but the embodiments do not limit the present invention in any form.
[0061] In the embodiments and comparative examples of the present invention, polylactic acid (hereinafter referred to as PLA for ease of description) is homemade, and the preparation method is: lactic acid monomer and initiator (glycerol) are mixed, and then a catalyst is added, and a polymerization reaction is carried out at a temperature of 120 to 160° C. and a vacuum degree of -0.050 to -0.09 MPa. The reaction time is 10 to 25 hours to obtain PLA. Different viscosities have been obtained by controlling different reaction times or different amounts of initiators added.
[0062] Among them: PLA-1, viscosity is 0.5dL / g, D-type content is 0.5%, and melting point is 176°C; PLA-2, viscosity is 1.0dL / g, D-type content is 0.8%, and melting point is 170°C; PLA-3, viscosity is 0.2dL / g, D-type content is 1.0%, and melting point is 165°C; PLA-4, viscosity is 1.2dL / g, D-type content is 1.2%, and melting point is 154°C.
[0063] Unless otherwise specified, the reagents, methods and equipment used in the present invention are conventional reagents, methods and equipment in the art. Unless otherwise specified, the reagents and materials used in the present invention are commercially available.
[0064] Examples 1 to 6
[0065] Examples 1 to 6 respectively provide a biodegradable polyester copolymer, and the preparation method is as follows:
[0066] S1. 166 kg of terephthalic acid and 105 kg of 1,4-butanediol were mixed to obtain a mixture A; 3.5 kg of 1,4-butanediol was mixed with 0.2 kg of a catalyst (n-butyl titanate) to obtain a mixture B, and then the mixture A and the mixture B were added to an esterification reaction device, respectively, to carry out an esterification reaction, and obtain an esterified product E1;
[0067] S2. 144 kg of adipic acid and 100 kg of 1,4-butanediol were mixed, and the resulting mixture was added to an esterification reaction apparatus to perform an esterification reaction to obtain an esterified product E2;
[0068] S3 245kg ester E1, 210kg ester E2 and 152kg PLA-1 were mixed and added to a copolymerization reaction device to carry out a copolymerization reaction to obtain a biodegradable polyester copolymer;
[0069] That is, in this embodiment, based on the total molar amount of terephthalic acid and adipic acid, terephthalic acid accounts for 50 mol%, and adipic acid accounts for 50 mol%; based on the total amount of ester E1, ester E2 and PLA-1, the weight of PLA-1 accounts for 25 wt.%;
[0070] The specific reaction conditions are shown in Table 1.
[0071] Table 1
[0072]
[0073] Embodiments 7 to 9
[0074] Examples 7 to 9 respectively provide a biodegradable polyester copolymer, and the preparation method is different from that of Example 1 in that:
[0075] In Example 7, the addition amounts of terephthalic acid and adipic acid are adjusted to be controlled as follows: based on the total molar amount of terephthalic acid and adipic acid, terephthalic acid accounts for 40 mol % and adipic acid accounts for 60 mol %;
[0076] In Example 8, the amount of PLA added was adjusted to be controlled as follows: based on the total amount of ester E1, ester E2 and PLA, the weight of PLA accounted for 10 wt.%;
[0077] In Example 9, the amount of PLA added was adjusted to be controlled such that the weight of PLA accounted for 40 wt.% based on the total amount of ester E1, ester E2 and PLA;
[0078] Embodiments 10 to 12
[0079] Examples 10 to 12 respectively provide a biodegradable polyester copolymer, and the preparation method is the same as that of Example 1, except that:
[0080] In Example 10, PLA-1 was replaced by PLA-2 in equal amounts;
[0081] In Example 11, PLA-1 was replaced by PLA-3 in equal amounts;
[0082] In Example 12, PLA-1 was replaced by PLA-4 in equal amounts.
[0083] Comparative Example 1
[0084] Comparative Example 1 provides a biodegradable polyester copolymer, and the preparation method is different from that of Example 1 in that:
[0085] S1. 166 kg of terephthalic acid was mixed with 105 kg of 1,4-butanediol to obtain a mixture A; 3.5 kg of 1,4-butanediol was mixed with 0.2 kg of a catalyst (n-butyl titanate) to obtain a mixture B; 144 kg of adipic acid was mixed with 100 kg of 1,4-butanediol to obtain a mixture C;
[0086] Then, mixture A, mixture B and mixture C are added to the esterification reaction equipment respectively to carry out esterification reaction to obtain esterified product.
[0087] S3. 455 kg of the esterified product and 152 kg of PLA-1 were mixed and added to a copolymerization reaction device to carry out copolymerization to obtain a biodegradable polyester copolymer.
[0088] Comparative Examples 2 to 5
[0089] Comparative Examples 2 to 5 provide a biodegradable polyester copolymer. The preparation method is different from that of Example 1 in that: in step S1 and step S2, the terminal carboxyl content of the esterified product E1 and the esterified product E2 is controlled differently. The specific reaction conditions of step S1 and step S2 are shown in Table 2. Step S3 is the same as Example 1.
[0090] Table 2
[0091]
[0092]
[0093] Comparative Example 6
[0094] Comparative Example 6 provides a biodegradable polyester copolymer, the preparation method of which is as follows:
[0095] 90 kg PBAT (trade name A400, from Zhuhai Kingfa Biomaterials Co., Ltd.) and 30 kg PLA (trade name L175, from Total PLA) were mixed, and 0.3 kg compatibilizer (ADR 4368) was added. After mixing the components, they were added to a twin-screw extruder (L / D=48; diameter 40 mm) for melt mixing, extrusion and granulation. The extrusion temperature was 140-200°C, the screw speed was 300 rpm, and the vacuum was -0.50 to -0.65 kg / cm 2 , and obtain a biodegradable polyester copolymer.
[0096] Performance Testing
[0097] The biodegradable polyester copolymers prepared in the above examples and comparative examples were tested for performance, and the specific method is as follows:
[0098] Tensile strength: tested according to ISO 527-2-2012 standard method;
[0099] Elongation at break: tested according to ISO 527-2-2012 standard method;
[0100] Biodegradation rate: The biodegradable polyester copolymer was prepared into a 12 μm±1 μm film, and the biodegradation rate after being placed for 12 weeks was tested according to the standard ISO16929 (2013).
[0101] The test results are shown in Table 3.
[0102] Table 3
[0103]
[0104] According to the test results in Table 3, the biodegradable polyester copolymers prepared in various embodiments of the present invention have good mechanical properties. When the weight of PLA accounts for 25wt.%, the tensile strength of the biodegradable polyester copolymer is ≥33MPa, and the elongation at break is ≥198%. At the same time, the biodegradable polyester copolymers prepared in various embodiments also have good biodegradability.
[0105] According to Examples 1 to 6, it can be seen that when the terminal carboxyl content of the ester E1 obtained in step S1 is controlled to be 50 to 450 mol / t and the terminal carboxyl content of the ester E2 obtained in step S2 is controlled to be 500 to 5000 mol / t, the copolymerization reaction in step S3 can be effectively carried out, and the PLA phase in the obtained biodegradable polyester copolymer can be uniformly dispersed, so that the biodegradable polyester copolymer has good mechanical properties. When the terminal carboxyl content of the ester E1 is 100 to 400 mol / t and the terminal carboxyl content of the ester E2 is 2000 to 3000 mol / t, the mechanical properties of the obtained biodegradable polyester copolymer are relatively better, with a tensile strength of ≥37 MPa and an elongation at break of ≥250%.
[0106] According to Comparative Example 1, when the esterification reactions of the aromatic dicarboxylic acid compounds and the aliphatic dicarboxylic acid compounds are not controlled separately, it is difficult to obtain an ester with a suitable terminal carboxyl content, and the mechanical properties of the obtained biodegradable polyester copolymer are poor.
[0107] According to Comparative Examples 2 to 5, when the terminal carboxyl content of the esterified product E1 and the esterified product E2 exceeds the range defined in the present invention, the tensile strength and elongation at break of the obtained biodegradable polyester copolymer are significantly deteriorated.
[0108] According to Example 1 and Examples 10 to 12, when the viscosity of PLA is 0.2 to 1.0 dL / g, the copolymerization reaction in step S3 can be carried out efficiently, and the PLA phase in the biodegradable polyester copolymer is better dispersed, so that the mechanical properties of the biodegradable polyester copolymer are relatively better.
[0109] In Comparative Example 6, PBAT and PLA are directly blended. Even if a compatibilizer is added for melting, the morphology of the PBAT / PLA blend is still a phase separation structure, and the mechanical properties of the obtained biodegradable polyester copolymer are difficult to meet the requirements.
[0110] Finally, it should be noted that the above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the scope of protection of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.
Claims
1. A method for preparing a biodegradable polyester copolymer, It is characterized in that The steps include: S1. An aromatic dicarboxylic acid compound, 1,4-butanediol and a catalyst are mixed to perform an esterification reaction to obtain an esterified product E1, wherein the terminal carboxyl content of the esterified product E1 is 50 to 450 mol / t; S2. mixing an aliphatic dicarboxylic acid compound with 1,4-butanediol, and performing an esterification reaction to obtain an esterified product E2, wherein the terminal carboxyl content of the esterified product E2 is 500 to 5000 mol / t; S3. The esterified product E1, the esterified product E2 and the polylactic acid are mixed and added to a copolymerization reaction device, and reacted at 200-250° C. and 1000-5000 Pa for 1.5-4 h to obtain a biodegradable polyester copolymer. in, Based on the total molar amount of the aromatic dicarboxylic acid compound and the aliphatic dicarboxylic acid compound, the aromatic dicarboxylic acid compound accounts for 38 to 52 mol%, and the aliphatic dicarboxylic acid compound accounts for 48 to 62 mol%; The D-type content of the polylactic acid is 0.4-1.6%, and the melting point of the polylactic acid is 150-180°C.
2. The method for preparing the biodegradable polyester copolymer according to claim 1, It is characterized in that In step S1, the esterification reaction is carried out at 200-250° C. and 30-110 KPa for 1.5-3.5 hours.
3. The method for preparing the biodegradable polyester copolymer according to claim 1, It is characterized in that In step S2, the esterification reaction is carried out at 150-200° C. and 30-110 KPa for 2-4 hours.
4. The method for preparing the biodegradable polyester copolymer according to claim 1, It is characterized in that The aromatic dicarboxylic acid compound is at least one of terephthalic acid, dimethyl terephthalate, diethyl terephthalate, dibutyl terephthalate, dioctyl terephthalate, ethylene terephthalate, butylene terephthalate, isophthalic acid, dioctyl isophthalate, naphthalene dicarboxylic acid and diphenyl dicarboxylic acid.
5. The method for preparing the biodegradable polyester copolymer according to claim 1, It is characterized in that The aliphatic dicarboxylic acid compound is at least one of succinic acid, adipic acid, suberic acid and sebacic acid.
6. The method for preparing the biodegradable polyester copolymer according to claim 1, It is characterized in that The intrinsic viscosity of the polylactic acid is 0.2 to 1.2 dL / g.
7. The method for preparing the biodegradable polyester copolymer according to claim 1, It is characterized in that In step S3, the intrinsic viscosity of the biodegradable polyester copolymer is 1.2-1.8 dL / g.
8. The method for preparing the biodegradable polyester copolymer according to claim 1, It is characterized in that Based on the total amount of the ester E1, the ester E2 and the polylactic acid, the weight of the polylactic acid is 8 to 41 wt.%.
9. A biodegradable polyester copolymer prepared by the method according to any one of claims 1 to 8, It is characterized in that The difference η between the melting point corresponding to the polylactic acid component in the biodegradable polyester copolymer and the theoretical melting point of the biodegradable polyester copolymer is ≤22°C.
10. Use of the biodegradable polyester copolymer according to claim 9 in preparing disposable film bags.
Citation Information
Patent Citations
Fully degradable biomaterial and product thereof
CN102702696A
Unsaturated polylactic acid segmented copolymer and preparation method thereof
CN104725620A
Continuous production method for biodegradable aliphatic-aromatic copolyester
CN102443149A
Biodegradable aliphatic-aromatic copolyester and synthetic method thereof
CN114621420A
Low-carboxyl-terminated biodegradable polyester and preparation method of special material thereof
CN115286777A