Looseness and elasticity style finishing agent for chemical fibers and blended fabrics thereof and preparation method of looseness and elasticity style finishing agent

By mixing the polyurethane intermediate with crosslinked structures with polysiloxane, the existing terpolymer silicone oil finishing style single and single and single-siloxane by using trimethylolpropane, isocyanate, N,N-dimethylethanolamine, and methyl ethyl ketone oxime to prepare the crosslinked structure. The problem of insufficient washing resistance has achieved improved fluffy, elasticity and washing resistance of the fabric.

CN119081127APending Publication Date: 2024-12-06HUBEI XINGRUI SILICON MATERIAL CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411294463.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-14
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing terpolymer silicone oil has a single style when sorting fabrics, lacks fluffy and thick effects, and the finishing agent has insufficient washing resistance.

Method used

The polyurethane intermediate with crosslinked structure is prepared by trimethylolpropane, isocyanate, N,N-dimethylethanolamine, and methyl ethyl ketone oxime is mixed with polysiloxane to form a finishing agent with a crosslinking structure, and improve the crosslinking of the finishing agent. degree and fluffy effect, and enhance wash resistance through reactive group reaction.

Benefits of technology

It gives the fabric an excellent fluffy and elasticity, making the fabric full, rebound and thick style, while improving the washing resistance and finishing effect of the finishing agent.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_9
    Figure SMS_9
  • Figure SMS_16
    Figure SMS_16
Patent Text Reader

Abstract

The invention provides a loose elastic style finishing agent for chemical fibers and blended fabrics thereof and a preparation method of the loose elastic style finishing agent. Firstly, epoxy-terminated polyether silicone oil and polyether amine are adopted as raw materials, and a proper amount of solvent is added to synthesize block silicone oil; then, trimethylolpropane, diisocyanate, N, N-dimethylethanolamine and methyl ethyl ketoxime are adopted as raw materials, and N, N-dimethylformamide is adopted as a solvent to synthesize a polyurethane intermediate; and adding the polyurethane intermediate into block silicone oil, and emulsifying the system to obtain the loose and elastic style finishing agent for chemical fibers and blended fabrics thereof. The loose and elastic style finishing agent for the chemical fiber and the blended fabric of the chemical fiber combines the advantages of organic silicon and polyurethane, has a good loose and elastic style finishing effect and also has good washing resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of printing and dyeing auxiliaries, and specifically relates to a loose elastic finishing agent for chemical fiber and blended fabrics thereof and a preparation method thereof. Background Art

[0002] Softening finishing is a very important process after printing and dyeing. Polyether amino block copolymer silicone oil (hereinafter referred to as ternary copolymer silicone oil) is the most widely used softening finishing agent in softening finishing. At present, most ternary copolymer silicone oils use end-epoxy polyether silicone oil and polyether amine to undergo ring-opening reaction under appropriate conditions. The obtained product has the characteristics of self-emulsification, high adsorption, dryness and smoothness, and is suitable for ultra-smooth and soft finishing of cotton, chemical fiber and blended fabrics. Ternary copolymer silicone oil has many advantages, such as good stability, small batch difference, mild reaction conditions and can give fabrics excellent smoothness and softness. However, the ternary copolymer block silicone oil synthesized by this method is mostly a regular linear structure, and the finishing style of the fabric is relatively single, lacking fullness, thickness and other styles. Polyurethane is a polymer containing many carbamate groups generated by polymerization of diisocyanate or polyisocyanate and a substance with 2 or more active hydrogens. Polyurethane materials are usually composed of flexible segments (soft segments) and rigid segments (hard segments) with different glass transition temperatures. In terms of thermodynamics, the incompatibility between the hard segments with stronger polarity and the soft segments causes the hard segments to aggregate to form many micro-regions and distribute among the soft segments, thus forming a microphase separation structure, which gives polyurethane unique properties such as thermal stability and high elasticity.

[0003] Therefore, the present invention adopts trimethylolpropane, diisocyanate, N,N-dimethylethanolamine, and methyl ethyl ketone oxime to prepare a blocked polyurethane intermediate with a cross-linked structure and water solubility, and modifies the ternary copolymer block silicone oil to obtain a finishing agent that can give the fabric a fluffy and elastic style. In the baking stage of finishing, the active groups of the polyurethane intermediate are unblocked and react with the active groups on the ternary copolymer block silicone oil, thereby improving the cross-linking degree of the system; in addition, the cross-linked polyurethane intermediate itself has excellent elasticity. Therefore, the finishing agent prepared by the present invention can give the fabric excellent fluffy feeling and elasticity, so that the fabric has a full, resilient, and thick style. Summary of the invention

[0004] The present invention provides a finishing agent which can give chemical fiber and its blended fabric a good loose and elastic feel, and is obtained by mixing a polyurethane intermediate and polysiloxane; The structural formula of the polyurethane intermediate is:

[0005] or ; Among them, -R- represents , , , , , Any one of .

[0006] Furthermore, the polysiloxane is obtained by reacting terminal epoxy polyether silicone oil with polyether amine; and the mass ratio of the polysiloxane to the polyurethane intermediate is 208-555:1.

[0007] The present invention also provides a method for preparing a loose elastic finishing agent for chemical fiber and its blended fabrics, comprising the following steps: Preparation of polysiloxane: adding terminal epoxy polyether silicone oil, polyether amine and solvent into a reaction container, introducing nitrogen gas, and reacting to obtain polysiloxane; Preparation of polyurethane intermediates: (1) Trimethylolpropane and N,N-dimethylformamide are added to a reaction vessel, nitrogen is introduced, diisocyanate is added dropwise at a uniform rate, and then the reaction is carried out at a heat preservation temperature; (2) adding N,N-dimethylethanolamine based on step (1) and keeping the temperature to react; (3) adding methyl ethyl ketone oxime on the basis of step (2), and reacting at the same temperature. After the reaction is completed, N,N-dimethylformamide is removed by vacuum distillation to obtain a polyurethane intermediate; Preparation of the finishing agent: adding the polyurethane intermediate into polysiloxane, adding acetic acid, stirring and emulsifying, and obtaining a loose elastic finishing agent for chemical fiber and its blended fabrics.

[0008] The synthetic route of polyurethane intermediates is as follows:

[0009] Among them, -R- represents , , , , , Any one of .

[0010] Furthermore, the weight percentages of the raw materials for preparing polysiloxane are: 200-450 parts of terminal epoxy polyether silicone oil, 9-35 parts of polyether amine, and 141-306 parts of solvent; The mass parts of various raw materials for preparing the polyurethane intermediate are: 20 parts of trimethylolpropane, 75-120 parts of diisocyanate, 158-191 parts of N,N-dimethylformamide, 13-27 parts of N,N-dimethylethanolamine, and 12-26 parts of methyl ethyl ketone oxime.

[0011] Furthermore, the molecular weight of the epoxy-terminated polyether silicone oil is 7000-22000; the polyetheramine is one or more of polyetheramine D200, polyetheramine D400, polyetheramine ED600, polyetheramine ED900 or polyetheramine T403; and the solvent is one of isopropanol and ethylene glycol monobutyl ether.

[0012] Furthermore, the diisocyanate is one of hexamethylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane-4,4'-diisocyanate or isophorone isocyanate.

[0013] Furthermore, the preparation conditions of the polysiloxane are: reaction temperature is 80-85° C., and reaction time is 5-9 h.

[0014] Furthermore, in the preparation of the polyurethane intermediate: the reaction temperature of step (1) is 60-75°C, the reaction time is 3-4h, and the speed of uniformly adding diisocyanate is 0.5-3 seconds / drop; the reaction temperature of step (2) is 60-75°C, and the reaction time is 3-4h; the reaction temperature of step (3) is 75-85°C, and the reaction time is 2-4h.

[0015] Furthermore, in the preparation of the finishing agent, the stirring speed is 1000-1500 rpm.

[0016] The invention uses terminal epoxy polyether silicone oil and polyether amine to react in a proper amount of solvent for a certain period of time to obtain a polysiloxane product with a cross-linked structure, which can give fabrics a certain loose and elastic feel style; trimethylolpropane, diisocyanate and N,N-dimethylethanolamine are reacted in a proper amount of solvent for a certain period of time, and then methyl ethyl ketone oxime is used to block part of the remaining active isocyanate groups, so that the obtained polyurethane intermediate has a cross-linked structure and retains the active isocyanate groups.

[0017] The beneficial effects of the present invention are as follows: (1) The polyurethane intermediate is added to the polysiloxane. During the baking stage of the finishing process, the active isocyanate groups of the polyurethane intermediate are unblocked and react with the active groups on the ternary copolymer block silicone oil, thereby increasing the degree of cross-linking of the system. The polyurethane intermediate can also react with the active hydrogen groups on the fabric to improve the washability of the finishing agent. In addition, the polyurethane intermediate can also react with water during the baking process to generate carbon dioxide, further increasing the fluffiness of the finished product.

[0018] (2) The polyurethane intermediate has a three-pronged structure. When the polyurethane intermediate is added to polysiloxane for emulsification, the tertiary amine group at the end of the polyurethane intermediate reacts with the epoxy group on the polysiloxane, and the polysiloxane is grafted onto the three-pronged structure of the polyurethane intermediate, further enhancing the fluffy effect of the finishing agent.

[0019] (3) The polyurethane intermediate molecule contains an ester bond structure similar to that of chemical fiber. When baked at high temperature, the two will produce a eutectic phenomenon, which will increase the effect of the finishing agent on the fabric and at the same time improve the washability of the finishing effect.

[0020] (4) The polysiloxane prepared by the present invention contains a polyether segment, and the polyurethane intermediate contains a tertiary amine structure. Therefore, during emulsification, only a certain amount of acetic acid needs to be added, and no additional emulsifier needs to be added. The use is very convenient.

[0021] In summary, the elastic finishing agent for chemical fiber and its blended fabrics prepared by the present invention has a good finishing effect and meets the requirements of environmental protection regulations. DETAILED DESCRIPTION

[0022] The embodiments of the present invention will be described in detail below with reference to examples. The following examples are only used to illustrate the present invention and should not be construed as limiting the scope of the present invention.

[0023] Example 1 (1) 300 g of terminal epoxy polyether silicone oil with a molecular weight of 17,000, 15.88 g of polyetheramine ED600, and 210.58 g of isopropanol were added to a reaction vessel equipped with a stirrer, a thermometer, and a condensation reflux device, nitrogen was introduced, stirring and the condensation reflux device were turned on, the temperature was raised to 80° C., and the reaction was kept at this temperature for 5 hours to obtain polysiloxane; 20g of trimethylolpropane and 183.64g of N,N-dimethylformamide were added to a reaction vessel equipped with a stirrer, a thermometer, a constant pressure dropping funnel and a condensation reflux device, nitrogen was introduced, stirring and the condensation reflux device were turned on, the temperature was raised to 60°C, 76.46g of hexamethylene diisocyanate was added dropwise at a uniform speed within 10min, and the reaction was kept warm at 60°C for 3h; keeping the temperature unchanged, 13.28g of N,N-dimethylethanolamine was added to the reaction vessel, and the reaction was kept warm for 3h; the temperature was adjusted to 75°C, 25.97g of methyl ethyl ketone oxime was added to the reaction vessel, and the reaction was kept warm at 75°C for 2h, and then N,N-dimethylformamide was removed by reduced pressure distillation under the conditions of vacuum degree -0.1MPa and temperature 120°C to obtain a polyurethane intermediate.

[0024] (2) 0.95 g of the polyurethane intermediate was added to 526.46 g of polysiloxane, and 7.9 g of acetic acid was added. The mixture was stirred and emulsified at a speed of 1000 rpm to obtain a loose elastic finishing agent for chemical fiber and blended fabrics.

[0025] Example 2 (1) Add 200 g of terminal epoxy polyether silicone oil with a molecular weight of 22,000, 12.27 g of polyetheramine ED900, and 141.51 g of ethylene glycol monobutyl ether into a reaction vessel equipped with a stirrer, a thermometer, and a condensation reflux device, introduce nitrogen, start stirring and the condensation reflux device, raise the temperature to 82° C., and keep the temperature for 6 hours to obtain polysiloxane; 20g of trimethylolpropane and 161.62g of N,N-dimethylformamide were added to a reaction vessel equipped with a stirrer, a thermometer, a constant pressure dropping funnel and a condensation reflux device, nitrogen was introduced, stirring and the condensation reflux device were turned on, the temperature was raised to 65°C, 101.29g of isophorone diisocyanate was added dropwise at a uniform rate within 12min, and the reaction was kept warm at 65°C for 3.5h; keeping the temperature unchanged, 26.57g of N,N-dimethylethanolamine was added to the reaction vessel, and the reaction was kept warm for 3.5h; the temperature was adjusted to 80°C, 12.98g of methyl ethyl ketone oxime was added to the reaction vessel, and the reaction was kept warm at 80°C for 3h, and then N,N-dimethylformamide was removed by reduced pressure distillation under the conditions of vacuum degree -0.1MPa and temperature 120°C to obtain a polyurethane intermediate.

[0026] (2) 1.06 g of the polyurethane intermediate was added to 353.78 g of polysiloxane, and 5.31 g of acetic acid was added. The mixture was stirred and emulsified at a speed of 1200 rpm to obtain a loose elastic finishing agent for chemical fiber and blended fabrics.

[0027] Example 3 (1) Add 250 g of terminal epoxy polyether silicone oil with a molecular weight of 12,000, 13.87 g of polyetheramine T403, and 175.91 g of isopropanol into a reaction vessel equipped with a stirrer, a thermometer, and a condensation reflux device, introduce nitrogen, start stirring and the condensation reflux device, raise the temperature to 83°C, and keep the temperature for 7 hours to obtain polysiloxane; 20g of trimethylolpropane and 158.52g of N,N-dimethylformamide were added to a reaction vessel equipped with a stirrer, a thermometer, a constant pressure dropping funnel and a condensation reflux device, nitrogen was introduced, stirring and the condensation reflux device were turned on, the temperature was raised to 70°C, 79.18g of toluene diisocyanate was added dropwise at a uniform rate within 18min, and the reaction was kept warm at 70°C for 3.8h; keeping the temperature unchanged, 13.28g of N,N-dimethylethanolamine was added to the reaction vessel, and the reaction was kept warm for 3.8h; the temperature was adjusted to 85°C, 25.97g of methyl ethyl ketone oxime was added to the reaction vessel, and the reaction was kept warm at 85°C for 3.5h, and then N,N-dimethylformamide was removed by reduced pressure distillation under the conditions of vacuum degree -0.1MPa and temperature 120°C to obtain a polyurethane intermediate.

[0028] (2) 1.58 g of the polyurethane intermediate was added to 439.78 g of polysiloxane, and 6.6 g of acetic acid was added. The mixture was stirred and emulsified at a speed of 1500 rpm to obtain a loose elastic finishing agent for chemical fiber and blended fabrics.

[0029] Example 4 (1) 400 g of 7000 molecular weight epoxy-terminated polyether silicone oil, 34.28 g of polyetheramine D400, and 289.52 g of ethylene glycol monobutyl ether were added to a reaction vessel equipped with a stirrer, a thermometer, and a condensation reflux device, nitrogen was introduced, stirring and the condensation reflux device were turned on, the temperature was raised to 84° C., and the reaction was kept at this temperature for 8 hours to obtain polysiloxane; 20g of trimethylolpropane and 190.71g of N,N-dimethylformamide were added to a reaction vessel equipped with a stirrer, a thermometer, a constant pressure dropping funnel and a condensation reflux device, nitrogen was introduced, stirring and the condensation reflux device were turned on, the temperature was raised to 75°C, and 113.78g of diphenylmethane diisocyanate was added dropwise at a uniform speed within 20min, and the reaction was kept warm at 75°C for 4h; keeping the temperature unchanged, 26.57g of N,N-dimethylethanolamine was added to the reaction vessel, and the reaction was kept warm for 4h; the temperature was adjusted to 80°C, 12.98g of methyl ethyl ketone oxime was added to the reaction vessel, and the reaction was kept warm at 80°C for 4h, and then N,N-dimethylformamide was removed by reduced pressure distillation under the conditions of vacuum degree -0.1MPa and temperature 120°C to obtain a polyurethane intermediate.

[0030] (2) 3.04 g of the polyurethane intermediate was added to 723.8 g of polysiloxane, and 10.86 g of acetic acid was added. The mixture was stirred and emulsified at a speed of 1300 rpm to obtain a loose elastic finishing agent for chemical fiber and blended fabrics.

[0031] Example 5 (1) Add 450 g of terminal epoxy polyether silicone oil with a molecular weight of 15,000, 9 g of polyetheramine D200, and 306 g of isopropanol into a reaction vessel equipped with a stirrer, a thermometer, and a condensation reflux device, introduce nitrogen, start stirring and the condensation reflux device, raise the temperature to 85° C., and keep the temperature for 9 hours to obtain polysiloxane; 20g of trimethylolpropane and 184.25g of N,N-dimethylformamide were added to a reaction vessel equipped with a stirrer, a thermometer, a constant pressure dropping funnel and a condensation reflux device, nitrogen was introduced, stirring and the condensation reflux device were turned on, the temperature was raised to 68°C, and 119.25g of hydrogenated phenylmethane diisocyanate was added dropwise at a uniform speed within 14min, and the reaction was kept warm at 68°C for 3.2h; keeping the temperature unchanged, 13.28g of N,N-dimethylethanolamine was added to the reaction vessel, and the reaction was kept warm for 3.2h; the temperature was adjusted to 83°C, 25.97g of methyl ethyl ketone oxime was added to the reaction vessel, and the reaction was kept warm at 83°C for 3.6h, and then N,N-dimethylformamide was removed by reduced pressure distillation under the conditions of vacuum degree -0.1MPa and temperature 120°C to obtain a polyurethane intermediate.

[0032] (2) 3.67 g of the polyurethane intermediate was added to 765 g of polysiloxane, and 11.47 g of acetic acid was added. The mixture was stirred and emulsified at a speed of 1400 rpm to obtain a loose elastic finishing agent for chemical fiber and blended fabrics.

[0033] Comparative Example 1 (1) 300 g of terminal epoxy polyether silicone oil with a molecular weight of 17,000, 15.88 g of polyetheramine ED600, and 210.58 g of isopropanol were added to a reaction vessel equipped with a stirrer, a thermometer, and a condensation reflux device, nitrogen was introduced, stirring and the condensation reflux device were turned on, the temperature was raised to 80° C., and the reaction was kept at this temperature for 5 hours to obtain polysiloxane; 20g of trimethylolpropane and 183.64g of N,N-dimethylformamide were added to a reaction vessel equipped with a stirrer, a thermometer, a constant pressure dropping funnel and a condensation reflux device, nitrogen was introduced, stirring and the condensation reflux device were turned on, the temperature was raised to 60°C, 76.46g of hexamethylene diisocyanate was added dropwise at a uniform speed within 10min, and the reaction was kept warm at 60°C for 3h; keeping the temperature unchanged, 13.28g of N,N-dimethylethanolamine was added to the reaction vessel, and the reaction was kept warm for 3h; the temperature was adjusted to 75°C, 25.97g of methyl ethyl ketone oxime was added to the reaction vessel, and the reaction was kept warm at 75°C for 2h, and then N,N-dimethylformamide was removed by reduced pressure distillation under the conditions of vacuum degree -0.1MPa and temperature 120°C to obtain a polyurethane intermediate.

[0034] (2) 3.16 g of the polyurethane intermediate was added to 526.46 g of polysiloxane, and 7.9 g of acetic acid was added. The mixture was stirred and emulsified at a speed of 1000 rpm to obtain a loose elastic finishing agent for chemical fiber and blended fabrics.

[0035] Comparative Example 2 (1) 300 g of terminal epoxy polyether silicone oil with a molecular weight of 17,000, 15.88 g of polyetheramine ED600, and 210.58 g of isopropanol were added to a reaction vessel equipped with a stirrer, a thermometer, and a condensation reflux device, nitrogen was introduced, stirring and the condensation reflux device were turned on, the temperature was raised to 80° C., and the reaction was kept at this temperature for 5 hours to obtain polysiloxane; 20g of trimethylolpropane and 183.64g of N,N-dimethylformamide were added to a reaction vessel equipped with a stirrer, a thermometer, a constant pressure dropping funnel and a condensation reflux device, nitrogen was introduced, stirring and the condensation reflux device were turned on, the temperature was raised to 60°C, 76.46g of hexamethylene diisocyanate was added dropwise at a uniform speed within 10min, and the reaction was kept warm at 60°C for 3h; keeping the temperature unchanged, 13.28g of N,N-dimethylethanolamine was added to the reaction vessel, and the reaction was kept warm for 3h; the temperature was adjusted to 75°C, 25.97g of methyl ethyl ketone oxime was added to the reaction vessel, and the reaction was kept warm at 75°C for 2h, and then N,N-dimethylformamide was removed by reduced pressure distillation under the conditions of vacuum degree -0.1MPa and temperature 120°C to obtain a polyurethane intermediate.

[0036] (2) 0.47 g of the polyurethane intermediate was added to 526.46 g of polysiloxane, and 7.9 g of acetic acid was added. The mixture was stirred and emulsified at a speed of 1000 rpm to obtain a loose elastic finishing agent for chemical fiber and blended fabrics.

[0037] Comparative Example 3 (1) 300 g of terminal epoxy polyether silicone oil with a molecular weight of 17,000, 15.88 g of polyetheramine ED600, and 210.58 g of isopropanol were added to a reaction vessel equipped with a stirrer, a thermometer, and a condensation reflux device, nitrogen was introduced, stirring and the condensation reflux device were turned on, the temperature was raised to 80° C., and the reaction was kept at this temperature for 5 hours to obtain polysiloxane; 20g of trimethylolpropane and 183.64g of N,N-dimethylformamide were added to a reaction vessel equipped with an agitator, a thermometer, a constant pressure dropping funnel and a condensation reflux device, nitrogen was introduced, stirring and the condensation reflux device were turned on, the temperature was raised to 60°C, 71.98g of hexamethylene diisocyanate was added dropwise at a uniform speed within 10min, and the reaction was kept warm at 60°C for 3h; keeping the temperature unchanged, 13.28g of N,N-dimethylethanolamine was added to the reaction vessel, and the reaction was kept warm for 3h; the temperature was adjusted to 75°C, 25.97g of methyl ethyl ketone oxime was added to the reaction vessel, and the reaction was kept warm at 75°C for 2h, and then N,N-dimethylformamide was removed by reduced pressure distillation under the conditions of vacuum degree -0.1MPa and temperature 120°C to obtain a polyurethane intermediate.

[0038] (2) 0.95 g of the polyurethane intermediate was added to 526.46 g of polysiloxane, and 7.9 g of acetic acid was added. The mixture was stirred and emulsified at a speed of 1000 rpm to obtain a loose elastic finishing agent for chemical fiber and blended fabrics.

[0039] Polyester fabric and nylon fabric were used as samples to be treated, and the polyester fabric and nylon fabric were treated with the elastic finishing agent for chemical fiber provided in Examples 1 to 5 and Comparative Examples 1 to 3 of the present invention, respectively.

[0040] 1. Finishing process Fabrics used: polyester fabric, nylon fabric Finishing process: Dipping finishing liquid (loose elastic finishing agent content 20g / L) 1min → double dipping and double rolling (rolling rate 70%) → Pre-baking (100℃, 15min) → Baking (180℃, 2min) → Standing for 24h (Relative humidity 50%, 25℃) →Water washing 2. Test methods and standards The compression properties of polyester fabrics and nylon fabrics are tested according to FZ / T01054.1-1999 "General Principles of Fabric Style Test Methods" using FB-AUTO-A KES fabric style tester. A 20cm×20cm sample is taken and tested after pretreatment for 48 hours at a temperature of 20±2℃ and a relative humidity of 65%±2%.

[0041] The whiteness of polyester fabrics and nylon fabrics is tested with reference to GB / T8424.2-2001 “Instrumental method for evaluation of relative whiteness of textile colour fastness tests”.

[0042] The warp-direction wrinkle recovery angle of polyester fabric and pure cotton fabric is tested with reference to GB / T3819-1997 “Determination of Crease Recovery of Textile Fabrics”.

[0043] The washability of the finishing effect was tested in a SW-12A washfastness tester in accordance with GB / T8629-2017 "Household Washing and Drying Procedures for Textile Testing". The fabric was soaked in soap solution (soap detergent 2g / L), washed with shaking water at 40°C for 10 minutes, and then washed with clean water for 2 minutes, completing one wash, and a total of 5 washes.

[0044] See Table 1 for the performance test comparison results of polyester fabrics after finishing with the elastic finishing agents prepared in Examples 1 to 5 of the present invention and Comparative Examples 1 to 3.

[0045] See Table 2 for the performance test comparison results of nylon fabrics subjected to style finishing using the elastic style finishing agents prepared in Examples 1 to 5 of the present invention and Comparative Examples 1 to 3.

[0046]

[0047] Table 1 Comparison results of performance test of polyester fabric before and after finishing Table 2 Comparison results of performance tests of nylon fabrics before and after finishing

[0048] In Examples 1 to 5, the proportion of polyurethane intermediates in the solid content of polysiloxane is getting larger and larger. From the data, it can be seen that the compression work ratio of polyester and nylon is also getting larger and larger, indicating that within a certain range, with the increase in the amount of polyurethane intermediates, the fluffiness and elasticity of the finished fabric are getting better and better. Too little (Comparative Example 1) or too much (Comparative Example 2) of the polyurethane intermediate will make the finishing effect of the finishing agent unsatisfactory. If the amount of polyurethane intermediate is too small, the finishing effect is not obvious. If the amount is too large, the molecules of the finishing agent will be cross-linked, resulting in difficulty in emulsification, making it difficult for the finishing agent to be finished on the fabric. In Comparative Example 3, trimethylolpropane is excessive relative to diisocyanate, resulting in some molecules being hydroxyl-terminated instead of active isocyanate-terminated, so the finishing effect will be reduced.

Claims

1. A loose elastic finishing agent for chemical fiber and its blended fabrics, characterized in that: It is obtained by mixing a polyurethane intermediate with polysiloxane; The structural formula of the polyurethane intermediate is: or ; Among them, -R- represents , , , , , Any one of .

2. The elastic finishing agent for chemical fiber and its blended fabrics according to claim 1, characterized in that: The polysiloxane is obtained by reacting terminal epoxy polyether silicone oil with polyether amine; and the mass ratio of the polysiloxane to the polyurethane intermediate is 208-555:

1.

3. A method for preparing a loose elastic finishing agent for chemical fiber and its blended fabrics, characterized in that: The following steps are involved: Preparation of polysiloxane: adding terminal epoxy polyether silicone oil, polyether amine and solvent into a reaction container, introducing nitrogen gas, and reacting to obtain polysiloxane; Preparation of polyurethane intermediates: (1) Trimethylolpropane and N,N-dimethylformamide are added to a reaction vessel, nitrogen is introduced, diisocyanate is added dropwise at a uniform rate, and then the reaction is carried out at a heat preservation temperature; (2) adding N,N-dimethylethanolamine based on step (1) and keeping the temperature to react; (3) adding methyl ethyl ketone oxime on the basis of step (2), and reacting at the same temperature. After the reaction is completed, N,N-dimethylformamide is removed by vacuum distillation to obtain a polyurethane intermediate; Preparation of the finishing agent: adding the polyurethane intermediate into polysiloxane, adding acetic acid, stirring and emulsifying, and obtaining a loose elastic finishing agent for chemical fiber and its blended fabrics.

4. The method for preparing a loose elastic finishing agent for chemical fiber and its blended fabrics according to claim 3, characterized in that: The weight proportions of the raw materials for preparing polysiloxane are as follows: 200-450 parts of terminal epoxy polyether silicone oil, 9-35 parts of polyether amine, and 141-306 parts of solvent; The mass parts of various raw materials for preparing the polyurethane intermediate are: 20 parts of trimethylolpropane, 75-120 parts of diisocyanate, 158-191 parts of N,N-dimethylformamide, 13-27 parts of N,N-dimethylethanolamine, and 12-26 parts of methyl ethyl ketone oxime.

5. The method for preparing a loose elastic finishing agent for chemical fiber and its blended fabrics according to claim 3, characterized in that: The molecular weight of the epoxy-terminated polyether silicone oil is 7000-22000; the polyetheramine is one or more of polyetheramine D200, polyetheramine D400, polyetheramine ED600, polyetheramine ED900 or polyetheramine T403; and the solvent is one of isopropanol and ethylene glycol monobutyl ether.

6. The method for preparing a loose elastic finishing agent for chemical fiber and its blended fabrics according to claim 3, characterized in that: The diisocyanate is one of hexamethylene diisocyanate, toluene diisocyanate, diphenylmethane diisocyanate, dicyclohexylmethane-4,4'-diisocyanate or isophorone isocyanate.

7. The method for preparing a loose elastic finishing agent for chemical fiber and its blended fabrics according to claim 3, characterized in that: The preparation conditions of the polysiloxane are: reaction temperature is 80-85° C., and reaction time is 5-9 h.

8. The method for preparing a loose elastic finishing agent for chemical fiber and its blended fabrics according to claim 3, characterized in that: In the preparation of the polyurethane intermediate: the reaction temperature of step (1) is 60-75°C, the reaction time is 3-4h, and the speed of uniformly adding diisocyanate is 0.5-3 seconds / drop; the reaction temperature of step (2) is 60-75°C, and the reaction time is 3-4h; the reaction temperature of step (3) is 75-85°C, and the reaction time is 2-4h.

9. The method for preparing a loose elastic finishing agent for chemical fiber and its blended fabrics according to claim 3, characterized in that: In the preparation of the finishing agent, the stirring speed is 1000-1500 rpm.