Lignin-based high internal phase Pickering emulsion and preparation method thereof
Through the combination of spherical lignin nanoparticles and PVP, a stable O/W high internal phase Pickering emulsion was prepared by utilizing the depletion attraction effect of high polymer level, which solved the problem that unmodified lignin nanoparticles were difficult to form a stable emulsion. , achieving excellent stability and environmentally friendly preparation technology under high oil load.
Patent Information
- Application Number
- CN202411369289.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-29
AI Technical Summary
Unmodified lignin nanoparticles are difficult to form stable O/W high internal phase Pickering emulsions, and chemical modification treatment is complex and may lead to environmental pollution.
Using spherical lignin nanoparticles and polyvinylpyrrolidone PVP as stabilizers, O/W oil-in-water high internal phase Pickering emulsion was prepared through homogeneous emulsification technology, and the stability of droplets was achieved by using the depletion attraction effect of high polymer levels. .
With high oil load and low stabilization agent addition, the excellent storage stability of the emulsion is achieved, and the preparation process is simple, low cost and environmentally friendly. It is suitable for the food industry, drug delivery, materials science and other fields.
Smart Images

Figure CN119081151A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of Pickering emulsions, and in particular relates to a lignin-based high internal phase Pickering emulsion and a preparation method thereof. Background Art
[0002] High internal phase emulsion (HIPE) is usually called super concentrated emulsion, which contains dispersed phase, continuous phase and necessary stabilizers to maintain the dynamic stability of the system. The volume fraction of the dispersed phase of the general emulsion is 30-50%, and the dispersed phase is dispersed in the continuous phase as unconnected spherical droplets; when the volume fraction of the dispersed phase reaches the critical density of 74.05%, the dispersed phase liquid will be tightly packed into interconnected spheres; further increase the volume fraction of the dispersed phase, the dispersed phase droplets will squeeze each other and deform into polygons. At this time, the emulsion with a dispersed phase volume fraction of more than 74.05% is a high internal phase emulsion. Due to its high load capacity and special rheological behavior, high internal phase emulsions are widely used in drug formulation, tissue engineering, food and other fields.
[0003] When using small molecule surfactants as stabilizers to stabilize high internal phase emulsions, due to the kinetically unstable nature of the small molecule surfactants themselves, they have weak adhesion at the oil-water interface and are easily lost. Therefore, a large amount of stabilizers is generally required to stabilize the high internal phase emulsions. Such a large amount of surfactants constitutes a potential environmental defect. In recent years, small molecule surfactants have been gradually replaced by amphiphilic biomacromolecules and organic or inorganic solid particles. In high internal phase Pickering emulsions (HIPPE) stabilized by solid particles, the particles are irreversibly adsorbed on the oil-water interface, reducing the total free energy and generating a strong interfacial mechanical barrier. The adsorbed particles wrap the droplets, making the emulsion highly stable against aggregation and Ostwald ripening.
[0004] Lignin is a heterogeneous, amorphous phenolic polymer. The non-polar aromatic and polar hydroxyl groups in its macromolecules make lignin particles naturally amphiphilic, so lignin nanoparticles are ideal candidate stabilizers for O / W Pickering emulsions. However, when unmodified lignin nanoparticles are used to prepare O / W high internal phase Pickering emulsions, the oil droplets formed are large and polydisperse, and the number of particles that can be used to stabilize the emulsion is small. The stable particles cannot fully cover more droplet surfaces, causing some droplets in the emulsion to aggregate into larger droplets during the emulsification process, and it is impossible to obtain a stable O / W high internal phase Pickering emulsion.
[0005] However, chemical modification of lignin makes the emulsion preparation process more complicated, and the use of chemical reagents also has potential environmental pollution. Therefore, the use of unmodified lignin nanoparticles to produce stable O / W high internal phase Pickering emulsions is still a problem to be solved in the field. Summary of the invention
[0006] In order to solve the problem that a stable O / W high internal phase Pickering emulsion cannot be obtained by using unmodified lignin nanoparticles as a stabilizer, the present invention provides a lignin-based high internal phase Pickering emulsion and a preparation method thereof.
[0007] The technical solution of the present invention:
[0008] A lignin-based high internal phase Pickering emulsion is an O / W oil-in-water emulsion, wherein the water phase is an ultrapure water suspension containing spherical lignin nanoparticles and polyvinylpyrrolidone (PVP), and the volume ratio of the water phase to the oil phase is 25:75.
[0009] Furthermore, the mass percentage of spherical lignin nanoparticles in the lignin-based high internal phase Pickering emulsion is 0.25%, and the mass percentage of PVP is 0.025-2.5%.
[0010] Furthermore, the spherical lignin nanoparticles have an average particle size of 146.1±0.6 nm, are monodisperse, and have a PDI of 0.061.
[0011] Furthermore, the molecular weight of the PVP is 40,000.
[0012] Furthermore, the oil phase is one of non-edible polar oil, non-edible non-polar oil or edible oil.
[0013] A method for preparing a lignin-based high internal phase Pickering emulsion comprises the steps of adding spherical lignin nanoparticles and PVP into ultrapure water to obtain an ultrapure water suspension; mixing the ultrapure water suspension with an oil phase and homogenizing and emulsifying the mixture to obtain the lignin-based high internal phase Pickering emulsion.
[0014] Furthermore, the preparation method of the spherical lignin nanoparticles is to dissolve the sulfate lignin in a tetrahydrofuran aqueous solution with a mass concentration of 50 to 90% at a mass ratio of 1:10 to 500, and filter and collect the purified lignin solution; add 2 to 5 times the mass of ultrapure water to the obtained purified lignin solution at a stirring speed of 800 to 2000 rpm, evaporate and remove tetrahydrofuran, and concentrate and filter the obtained suspension to obtain spherical lignin nanoparticles.
[0015] Furthermore, the mass concentration of the spherical lignin nanoparticles in the ultrapure water suspension is 1 wt %.
[0016] Furthermore, the mass concentration of PVP in the ultrapure water suspension is 0.1-10 wt %.
[0017] Furthermore, the rotation speed of the homogenization and emulsification is 8000-12000 rpm, and the time of the homogenization and emulsification is 3-4 minutes.
[0018] Beneficial effects of the present invention:
[0019] The lignin-based high internal phase Pickering emulsion provided by the present invention uses unmodified spherical lignin nanoparticles as a stabilizer, polyvinylpyrrolidone PVP as a dissipant, and utilizes the exhaustion attraction between the spherical lignin nanoparticles and droplets at a high polymer level, so that the structure of the flocculated droplets in the high internal phase emulsion system is exhausted and depleted to achieve exhaustion stabilization. The stability test results show that after the lignin-based high internal phase Pickering emulsion prepared by the present invention is stored undisturbed at room temperature for several weeks, no changes such as deoiling of the emulsion system are observed, which indicates that under the condition of high oil load and low stabilizer addition, the lignin-based high internal phase Pickering emulsion achieves excellent storage stability.
[0020] The preparation method of the lignin-based high internal phase Pickering emulsion of the present invention provides a simple green strategy, does not require modification of lignin nanoparticles, has a simple preparation process, low cost, and is environmentally friendly. The prepared high internal phase Pickering emulsion has broad application prospects in the fields of food industry, drug delivery, material science, cosmetics, oil extraction, and environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS
[0021] Figure 1 This is a morphology characterization photograph of the spherical lignin nanoparticles prepared in Example 1;
[0022] Figure 2 Fluorescence microscope photos of the lignin-based high internal phase Pickering emulsions prepared in Examples 1-8;
[0023] Figure 3 This is the appearance picture of the lignin-based high internal phase Pickering emulsion prepared in Example 1-8 on the first day of production;
[0024] Figure 4 This is the appearance of the lignin-based high internal phase Pickering emulsion prepared in Examples 1-8 after being stored at room temperature for 60 days. DETAILED DESCRIPTION
[0025] The technical solution of the present invention is further described below in conjunction with the embodiments, but it is not limited thereto. Any modification or equivalent replacement of the technical solution of the present invention without departing from the spirit and scope of the technical solution of the present invention shall be included in the protection scope of the present invention. The process equipment or devices not specifically noted in the following embodiments are all conventional equipment or devices in the art. If not specifically specified, the raw materials used in the embodiments of the present invention can be obtained commercially; if not specifically specified, the technical means used in the embodiments of the present invention are all conventional means well known to those skilled in the art.
[0026] Example 1
[0027] This embodiment provides a lignin-based high internal phase Pickering emulsion and a preparation method thereof.
[0028] In this embodiment, the lignin-based high internal phase Pickering emulsion is an O / W water-in-oil emulsion, and the volume ratio of the water phase to the oil phase is 25:75; the water phase is an ultrapure water suspension containing spherical lignin nanoparticles and polyvinylpyrrolidone PVP, and the oil phase is cyclohexane.
[0029] The mass percentage of spherical lignin nanoparticles in the lignin-based high internal phase Pickering emulsion of this embodiment is 0.25%, and the mass percentage of PVP is 0.025%. The average particle size of the spherical lignin nanoparticles in this embodiment is 146.1±0.6nm, monodisperse, and PDI is 0.061; the molecular weight of polyvinylpyrrolidone PVP is 40000.
[0030] The preparation method of the lignin-based high internal phase Pickering emulsion of this embodiment comprises the following steps:
[0031] Step 1: dissolve the kraft lignin in a tetrahydrofuran aqueous solution with a mass concentration of 75% at a mass ratio of 1:100, and stir overnight to completely dissolve it; filter with a filter paper with a pore size of 0.65 μm to remove insoluble lignin and impurities to obtain a purified lignin solution. Rapidly add ultrapure water 3 times the mass of the lignin solution to the purified lignin solution at a stirring speed of 2000 rpm, and the resulting precipitate is spherical lignin nanoparticles. Use a rotary evaporator to remove the residual tetrahydrofuran solvent, concentrate the resulting suspension, and filter with a filter paper with a pore size of 10 μm to remove deformed lignin nanoparticles and agglomerates to obtain spherical lignin nanoparticles.
[0032] Step 2: Add the spherical lignin nanoparticles and PVP obtained in step 1 into ultrapure water to obtain an ultrapure water suspension with a mass percentage of 1 wt% of spherical lignin nanoparticles and a mass percentage of 0.1 wt% of PVP; mix the obtained ultrapure water suspension with cyclohexane in a volume ratio of 25:75, and homogenize and emulsify at a speed of 10000 rpm for 4 minutes to obtain a lignin-based high internal phase Pickering emulsion.
[0033] Figure 1 The morphology characterization photo of the spherical lignin nanoparticles prepared in this embodiment; it can be seen from the figure that the obtained spherical lignin nanoparticles all present a uniform and smooth spherical structure, a small and uniform particle size, and a polydisperse system. The average particle size of the nanoparticles is 146.1±0.6nm, which is monodisperse, and the PDI is only 0.061. Due to the hydrophilic groups and negative electrostatic repulsion on the surface of the spherical lignin nanoparticles, the obtained spherical lignin nanoparticle dispersion can maintain colloidal stability within 6 months. The Zeta potential of SLN is around -40mV.
[0034] Example 2
[0035] This embodiment provides a lignin-based high internal phase Pickering emulsion and a preparation method thereof.
[0036] In this embodiment, the lignin-based high internal phase Pickering emulsion is an O / W water-in-oil emulsion, and the volume ratio of the water phase to the oil phase is 25:75; the water phase is an ultrapure water suspension containing spherical lignin nanoparticles and polyvinylpyrrolidone PVP, and the oil phase is cyclohexane.
[0037] The mass percentage of spherical lignin nanoparticles in the lignin-based high internal phase Pickering emulsion of this embodiment is 0.25%, the mass percentage of PVP is 0.25%, the mass percentage of oil phase is 75%, and the balance is ultrapure water. The average particle size of the spherical lignin nanoparticles in this embodiment is 146.1±0.6nm, monodisperse, and PDI is 0.061; the molecular weight of polyvinylpyrrolidone PVP is 40000.
[0038] The preparation method of the lignin-based high internal phase Pickering emulsion of this embodiment comprises the following steps:
[0039] Step 1: dissolve the kraft lignin in a tetrahydrofuran aqueous solution with a mass concentration of 75% at a mass ratio of 1:100, and stir overnight to completely dissolve it; filter with a filter paper with a pore size of 0.65 μm to remove insoluble lignin and impurities to obtain a purified lignin solution. Rapidly add ultrapure water 3 times the mass of the lignin solution to the purified lignin solution at a stirring speed of 2000 rpm, and the resulting precipitate is spherical lignin nanoparticles. Use a rotary evaporator to remove the residual tetrahydrofuran solvent, concentrate the resulting suspension, and filter with a filter paper with a pore size of 10 μm to remove deformed lignin nanoparticles and agglomerates to obtain spherical lignin nanoparticles.
[0040] Step 2: Add the spherical lignin nanoparticles and PVP obtained in step 1 into ultrapure water to obtain an ultrapure water suspension with a mass percentage of 1 wt% of spherical lignin nanoparticles and a mass percentage of 1 wt% of PVP; mix the obtained ultrapure water suspension with cyclohexane in a volume ratio of 25:75, and homogenize and emulsify at a speed of 10000 rpm for 4 minutes to obtain a lignin-based high internal phase Pickering emulsion.
[0041] Example 3
[0042] This embodiment provides a lignin-based high internal phase Pickering emulsion and a preparation method thereof.
[0043] In this embodiment, the lignin-based high internal phase Pickering emulsion is an O / W water-in-oil emulsion, and the volume ratio of the water phase to the oil phase is 25:75; the water phase is an ultrapure water suspension containing spherical lignin nanoparticles and polyvinylpyrrolidone PVP, and the oil phase is cyclohexane.
[0044] The mass percentage of spherical lignin nanoparticles in the lignin-based high internal phase Pickering emulsion of this embodiment is 0.25%, the mass percentage of PVP is 0.5%, the mass percentage of oil phase is 75%, and the balance is ultrapure water. The average particle size of the spherical lignin nanoparticles in this embodiment is 146.1±0.6nm, monodisperse, and PDI is 0.061; the molecular weight of polyvinylpyrrolidone PVP is 40000.
[0045] The preparation method of the lignin-based high internal phase Pickering emulsion of this embodiment comprises the following steps:
[0046] Step 1: dissolve the kraft lignin in a tetrahydrofuran aqueous solution with a mass concentration of 75% at a mass ratio of 1:100, and stir overnight to completely dissolve it; filter with a filter paper with a pore size of 0.65 μm to remove insoluble lignin and impurities to obtain a purified lignin solution. Rapidly add ultrapure water 3 times the mass of the lignin solution to the purified lignin solution at a stirring speed of 2000 rpm, and the resulting precipitate is spherical lignin nanoparticles. Use a rotary evaporator to remove the residual tetrahydrofuran solvent, concentrate the resulting suspension, and filter with a filter paper with a pore size of 10 μm to remove deformed lignin nanoparticles and agglomerates to obtain spherical lignin nanoparticles.
[0047] Step 2: Add the spherical lignin nanoparticles and PVP obtained in step 1 into ultrapure water to obtain an ultrapure water suspension with a mass percentage of 1 wt% of spherical lignin nanoparticles and a mass percentage of 2 wt% of PVP; mix the obtained ultrapure water suspension with cyclohexane in a volume ratio of 25:75, and homogenize and emulsify at a speed of 10,000 rpm for 4 minutes to obtain a lignin-based high internal phase Pickering emulsion.
[0048] Example 4
[0049] This embodiment provides a lignin-based high internal phase Pickering emulsion and a preparation method thereof.
[0050] In this embodiment, the lignin-based high internal phase Pickering emulsion is an O / W water-in-oil emulsion, and the volume ratio of the water phase to the oil phase is 25:75; the water phase is an ultrapure water suspension containing spherical lignin nanoparticles and polyvinylpyrrolidone PVP, and the oil phase is cyclohexane.
[0051] The mass percentage of spherical lignin nanoparticles in the lignin-based high internal phase Pickering emulsion of this embodiment is 0.25%, the mass percentage of PVP is 0.75%, the mass percentage of oil phase is 75%, and the balance is ultrapure water. The average particle size of the spherical lignin nanoparticles in this embodiment is 146.1±0.6nm, monodisperse, and PDI is 0.061; the molecular weight of polyvinylpyrrolidone PVP is 40000.
[0052] The preparation method of the lignin-based high internal phase Pickering emulsion of this embodiment comprises the following steps:
[0053] Step 1: dissolve the kraft lignin in a tetrahydrofuran aqueous solution with a mass concentration of 75% at a mass ratio of 1:100, and stir overnight to completely dissolve it; filter with a filter paper with a pore size of 0.65 μm to remove insoluble lignin and impurities to obtain a purified lignin solution. Rapidly add ultrapure water 3 times the mass of the lignin solution to the purified lignin solution at a stirring speed of 2000 rpm, and the resulting precipitate is spherical lignin nanoparticles. Use a rotary evaporator to remove the residual tetrahydrofuran solvent, concentrate the resulting suspension, and filter with a filter paper with a pore size of 10 μm to remove deformed lignin nanoparticles and agglomerates to obtain spherical lignin nanoparticles.
[0054] Step 2: Add the spherical lignin nanoparticles and PVP obtained in step 1 into ultrapure water to obtain an ultrapure water suspension with a mass percentage of 1 wt% of spherical lignin nanoparticles and a mass percentage of 3 wt% of PVP; mix the obtained ultrapure water suspension with cyclohexane in a volume ratio of 25:75, and homogenize and emulsify at a speed of 10,000 rpm for 4 minutes to obtain a lignin-based high internal phase Pickering emulsion.
[0055] Example 5
[0056] This embodiment provides a lignin-based high internal phase Pickering emulsion and a preparation method thereof.
[0057] In this embodiment, the lignin-based high internal phase Pickering emulsion is an O / W water-in-oil emulsion, and the volume ratio of the water phase to the oil phase is 25:75; the water phase is an ultrapure water suspension containing spherical lignin nanoparticles and polyvinylpyrrolidone PVP, and the oil phase is cyclohexane.
[0058] The mass percentage of spherical lignin nanoparticles in the lignin-based high internal phase Pickering emulsion of this embodiment is 0.25%, the mass percentage of PVP is 1%, the mass percentage of oil phase is 75%, and the balance is ultrapure water. The average particle size of the spherical lignin nanoparticles in this embodiment is 146.1±0.6nm, monodisperse, and PDI is 0.061; the molecular weight of polyvinylpyrrolidone PVP is 40000.
[0059] The preparation method of the lignin-based high internal phase Pickering emulsion of this embodiment comprises the following steps:
[0060] Step 1: dissolve the kraft lignin in a tetrahydrofuran aqueous solution with a mass concentration of 75% at a mass ratio of 1:100, and stir overnight to completely dissolve it; filter with a filter paper with a pore size of 0.65 μm to remove insoluble lignin and impurities to obtain a purified lignin solution. Rapidly add ultrapure water 3 times the mass of the lignin solution to the purified lignin solution at a stirring speed of 2000 rpm, and the resulting precipitate is spherical lignin nanoparticles. Use a rotary evaporator to remove the residual tetrahydrofuran solvent, concentrate the resulting suspension, and filter with a filter paper with a pore size of 10 μm to remove deformed lignin nanoparticles and agglomerates to obtain spherical lignin nanoparticles.
[0061] Step 2: Add the spherical lignin nanoparticles and PVP obtained in step 1 into ultrapure water to obtain an ultrapure water suspension with a mass percentage of 1 wt% of spherical lignin nanoparticles and a mass percentage of 4 wt% of PVP; mix the obtained ultrapure water suspension with cyclohexane in a volume ratio of 25:75, and homogenize and emulsify at a speed of 10,000 rpm for 4 minutes to obtain a lignin-based high internal phase Pickering emulsion.
[0062] Example 6
[0063] This embodiment provides a lignin-based high internal phase Pickering emulsion and a preparation method thereof.
[0064] In this embodiment, the lignin-based high internal phase Pickering emulsion is an O / W water-in-oil emulsion, and the volume ratio of the water phase to the oil phase is 25:75; the water phase is an ultrapure water suspension containing spherical lignin nanoparticles and polyvinylpyrrolidone PVP, and the oil phase is cyclohexane.
[0065] The mass percentage of spherical lignin nanoparticles in the lignin-based high internal phase Pickering emulsion of this embodiment is 0.25%, the mass percentage of PVP is 1.25%, the mass percentage of oil phase is 75%, and the balance is ultrapure water. The average particle size of the spherical lignin nanoparticles in this embodiment is 146.1±0.6nm, monodisperse, and PDI is 0.061; the molecular weight of polyvinylpyrrolidone PVP is 40000.
[0066] The preparation method of the lignin-based high internal phase Pickering emulsion of this embodiment comprises the following steps:
[0067] Step 1: dissolve the kraft lignin in a tetrahydrofuran aqueous solution with a mass concentration of 75% at a mass ratio of 1:100, and stir overnight to completely dissolve it; filter with a filter paper with a pore size of 0.65 μm to remove insoluble lignin and impurities to obtain a purified lignin solution. Rapidly add ultrapure water 3 times the mass of the lignin solution to the purified lignin solution at a stirring speed of 2000 rpm, and the resulting precipitate is spherical lignin nanoparticles. Use a rotary evaporator to remove the residual tetrahydrofuran solvent, concentrate the resulting suspension, and filter with a filter paper with a pore size of 10 μm to remove deformed lignin nanoparticles and agglomerates to obtain spherical lignin nanoparticles.
[0068] Step 2: Add the spherical lignin nanoparticles and PVP obtained in step 1 into ultrapure water to obtain an ultrapure water suspension with a mass percentage of 1 wt% of spherical lignin nanoparticles and a mass percentage of 5 wt% of PVP; mix the obtained ultrapure water suspension with cyclohexane in a volume ratio of 25:75, and homogenize and emulsify at a speed of 10,000 rpm for 4 minutes to obtain a lignin-based high internal phase Pickering emulsion.
[0069] Example 7
[0070] This embodiment provides a lignin-based high internal phase Pickering emulsion and a preparation method thereof.
[0071] In this embodiment, the lignin-based high internal phase Pickering emulsion is an O / W water-in-oil emulsion, and the volume ratio of the water phase to the oil phase is 25:75; the water phase is an ultrapure water suspension containing spherical lignin nanoparticles and polyvinylpyrrolidone PVP, and the oil phase is cyclohexane.
[0072] The mass percentage of spherical lignin nanoparticles in the lignin-based high internal phase Pickering emulsion of this embodiment is 0.25%, the mass percentage of PVP is 1.75%, the mass percentage of oil phase is 75%, and the balance is ultrapure water. The average particle size of the spherical lignin nanoparticles in this embodiment is 146.1±0.6nm, monodisperse, and PDI is 0.061; the molecular weight of polyvinylpyrrolidone PVP is 40000.
[0073] The preparation method of the lignin-based high internal phase Pickering emulsion of this embodiment comprises the following steps:
[0074] Step 1: dissolve the kraft lignin in a tetrahydrofuran aqueous solution with a mass concentration of 75% at a mass ratio of 1:100, and stir overnight to completely dissolve it; filter with a filter paper with a pore size of 0.65 μm to remove insoluble lignin and impurities to obtain a purified lignin solution. Rapidly add ultrapure water 3 times the mass of the lignin solution to the purified lignin solution at a stirring speed of 2000 rpm, and the resulting precipitate is spherical lignin nanoparticles. Use a rotary evaporator to remove the residual tetrahydrofuran solvent, concentrate the resulting suspension, and filter with a filter paper with a pore size of 10 μm to remove deformed lignin nanoparticles and agglomerates to obtain spherical lignin nanoparticles.
[0075] Step 2: Add the spherical lignin nanoparticles and PVP obtained in step 1 into ultrapure water to obtain an ultrapure water suspension with a mass percentage of 1 wt% of spherical lignin nanoparticles and a mass percentage of 7 wt% of PVP; mix the obtained ultrapure water suspension with cyclohexane in a volume ratio of 25:75, and homogenize and emulsify at a speed of 10,000 rpm for 4 minutes to obtain a lignin-based high internal phase Pickering emulsion.
[0076] Example 8
[0077] This embodiment provides a lignin-based high internal phase Pickering emulsion and a preparation method thereof.
[0078] In this embodiment, the lignin-based high internal phase Pickering emulsion is an O / W water-in-oil emulsion, and the volume ratio of the water phase to the oil phase is 25:75; the water phase is an ultrapure water suspension containing spherical lignin nanoparticles and polyvinylpyrrolidone PVP, and the oil phase is cyclohexane.
[0079] The mass percentage of spherical lignin nanoparticles in the lignin-based high internal phase Pickering emulsion of this embodiment is 0.25%, the mass percentage of PVP is 2.5%, the mass percentage of oil phase is 75%, and the balance is ultrapure water. The average particle size of the spherical lignin nanoparticles in this embodiment is 146.1±0.6nm, monodisperse, and PDI is 0.061; the molecular weight of polyvinylpyrrolidone PVP is 40000.
[0080] The preparation method of the lignin-based high internal phase Pickering emulsion of this embodiment comprises the following steps:
[0081] Step 1: dissolve the kraft lignin in a tetrahydrofuran aqueous solution with a mass concentration of 75% at a mass ratio of 1:100, and stir overnight to completely dissolve it; filter with a filter paper with a pore size of 0.65 μm to remove insoluble lignin and impurities to obtain a purified lignin solution. Rapidly add ultrapure water 3 times the mass of the lignin solution to the purified lignin solution at a stirring speed of 2000 rpm, and the resulting precipitate is spherical lignin nanoparticles. Use a rotary evaporator to remove the residual tetrahydrofuran solvent, concentrate the resulting suspension, and filter with a filter paper with a pore size of 10 μm to remove deformed lignin nanoparticles and agglomerates to obtain spherical lignin nanoparticles.
[0082] Step 2: Add the spherical lignin nanoparticles and PVP obtained in step 1 into ultrapure water to obtain an ultrapure water suspension with a mass percentage of 1 wt% of spherical lignin nanoparticles and a mass percentage of 10 wt% of PVP; mix the obtained ultrapure water suspension with cyclohexane in a volume ratio of 25:75, and homogenize and emulsify at a speed of 10000 rpm for 4 minutes to obtain a lignin-based high internal phase Pickering emulsion.
[0083] In order to verify the stability of the lignin-based high internal phase Pickering emulsion prepared by the present invention under a microscope, the microstructure of the lignin-based high internal phase Pickering emulsion was directly observed after being stained with an oil-soluble fluorescent dye using a fluorescence microscope. The results are as follows: Figure 2 shown. Figure 2 It shows that the size and distribution of oil droplets in the high internal phase Pickering emulsions prepared in Examples 1-8 with different PVP concentrations in the aqueous phase are uniform, and the proportional values shown in the figure are the mass percentage of PVP in the ultrapure water suspensions of Examples 1-8. When the PVP concentration in the aqueous phase increases from 0.1wt% to 3wt%, the average droplet diameter gradually decreases, and when the PVP concentration is greater than 3wt%, the average droplet diameter gradually increases.
[0084] Figure 3 This is the appearance of the lignin-based high internal phase Pickering emulsion prepared in Example 1-8 on the first day of production. The proportional values shown in the figure are the mass percentage of PVP in the ultrapure water suspension of Example 1-8; Figure 4This is an appearance picture of the lignin-based high internal phase Pickering emulsion prepared in Examples 1-8 after storage at room temperature for 60 days. The proportional values shown in the figure are the mass percentages of PVP in the ultrapure water suspensions of Examples 1-8. By comparison, it can be seen that after two months of undisturbed storage at room temperature, no changes such as deoiling of the emulsion system were observed for the lignin-based high internal phase Pickering emulsion prepared by the present invention. This indicates that under the conditions of high oil load and low stabilizer addition, the lignin-based high internal phase Pickering emulsion achieves excellent storage stability.
Claims
1. A lignin-based high internal phase Pickering emulsion, characterized in that: The lignin-based high internal phase Pickering emulsion is an O / W water-in-oil type emulsion, the water phase is an ultrapure water suspension containing spherical lignin nanoparticles and polyvinylpyrrolidone (PVP), and the volume ratio of the water phase to the oil phase is 25:
75.
2. A lignin-based high internal phase Pickering emulsion according to claim 1, characterized in that: The mass percentage of spherical lignin nanoparticles in the lignin-based high internal phase Pickering emulsion is 0.25%, and the mass percentage of PVP is 0.025-2.5%.
3. A lignin-based high internal phase Pickering emulsion according to claim 1 or 2, characterized in that: The spherical lignin nanoparticles have an average particle size of 146.1±0.6 nm, are monodisperse, and have a PDI of 0.
061.
4. A lignin-based high internal phase Pickering emulsion according to claim 3, characterized in that: The molecular weight of the PVP is 40,000.
5. A lignin-based high internal phase Pickering emulsion according to claim 4, characterized in that: The oil phase is one of non-edible polar oil, non-edible non-polar oil or edible oil.
6. A method for preparing a lignin-based high internal phase Pickering emulsion according to any one of claims 1 to 5, characterized in that: Spherical lignin nanoparticles and PVP are added into ultrapure water to obtain an ultrapure water suspension; the ultrapure water suspension is mixed with an oil phase and homogenized and emulsified to obtain a lignin-based high internal phase Pickering emulsion.
7. The method for preparing a lignin-based high internal phase Pickering emulsion according to claim 6, characterized in that: The preparation method of the spherical lignin nanoparticles comprises the following steps: dissolving kraft lignin in a tetrahydrofuran aqueous solution with a mass concentration of 50 to 90% at a mass ratio of 1:10 to 500, filtering and collecting the purified lignin solution; adding 2 to 5 times the mass of ultrapure water to the purified lignin solution at a stirring speed of 800 to 2000 rpm, evaporating and removing tetrahydrofuran, concentrating and filtering the obtained suspension to obtain the spherical lignin nanoparticles.
8. The method for preparing a lignin-based high internal phase Pickering emulsion according to claim 7, characterized in that: The mass concentration of the spherical lignin nanoparticles in the ultrapure water suspension is 1 wt %.
9. The method for preparing a lignin-based high internal phase Pickering emulsion according to claim 8, characterized in that: The mass concentration of PVP in the ultrapure water suspension is 0.1-10 wt %.
10. The method for preparing a lignin-based high internal phase Pickering emulsion according to claim 9, characterized in that: The rotation speed of the homogenization and emulsification is 8000-12000 rpm, and the time of the homogenization and emulsification is 3-4 minutes.
Citation Information
Patent Citations
Ultra-stable high-internal-phase Pickering emulsion gel as well as preparation method and application thereof
CN114907578A
Ultrahigh-salt-tolerance lignin-based Pickering emulsion and preparation method thereof
CN117801317A
Lignin-stabilized Pickering emulsion gel as well as preparation method and application thereof
CN117887101A
Cited By
Method for preparing immobilized lipase Janus particles by emulsion template one-step method and application of immobilized lipase Janus particles in Pickering emulsion catalysis
CN120041433A