Low-voltage cable containing modified graphene oxide and preparation method thereof
By using low-voltage cables containing modified graphene oxide in high-temperature and compressible cables, combined with hot-pressure forming process of materials such as phosphorus-containing modified benzooxazine, the problem of insufficient tensile performance of existing cables is solved. , achieving higher flame retardant effect and tensile performance.
Patent Information
- Application Number
- CN202411413724.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-12-06
AI Technical Summary
The existing high-temperature and compressive-resistant cables have shortcomings in tensile performance and are difficult to meet high-performance requirements.
Using low-voltage cables containing modified graphene oxide, the phosphorus-containing modified benzoxazine, modified graphene oxide, nano-aluminum hydroxide, polyethylene, maleic anhydride grafted polyethylene and calcium carbonate and other materials are used to graft the materials. The mixing machine is kneaded and hot-pressed in a flat vulcanizer to form a cable with excellent flame retardant and tensile properties.
It achieves good flame retardant and tensile performance, improves the thermal decomposition temperature and connection density of the cable, and significantly improves the overall performance of the cable.
Smart Images

Figure BDA0005078754230000081 
Figure BDA0005078754230000091
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cables, and in particular to a low-voltage cable containing modified graphene oxide and a preparation method thereof. Background Art
[0002] With the development of society, people's use of electricity is becoming more and more intense, and cables are indispensable for this. In practical applications, cables are not only used indoors, but also in more civil aviation fields. Therefore, the requirements for cable performance are also high. For example, patent CN10862042A discloses a high-temperature resistant and pressure-resistant cable sheath material and a preparation method thereof. The raw materials used in the invention are safe and environmentally friendly, the formula is scientific, the ratio is rigorous, the preparation method is simple, and it is easy to industrialize production, but its tensile properties are not improved. Summary of the invention
[0003] 1. Technical issues to be solved
[0004] In view of the deficiencies in the prior art, the present invention provides a low-voltage cable containing modified graphene oxide and a preparation method thereof, which has good flame retardancy and tensile properties.
[0005] (II) Technical solution
[0006] To achieve the above objectives, the present invention provides the following technical solutions: a low-voltage cable containing modified graphene oxide and a preparation method thereof, a low-voltage cable containing modified graphene oxide, comprising the following components by weight: 4-9 parts by weight of phosphorus-modified benzoxazine, 3-6 parts by weight of modified graphene oxide, 1-2 parts by weight of nano aluminum hydroxide, 75-90 parts by weight of polyethylene, 40-60 parts by weight of maleic anhydride grafted polyethylene, 1-2 parts by weight of calcium carbonate, and 0.2-0.4 parts by weight of antioxidant 1010.
[0007] Preferably, the preparation method of the phosphorus-modified benzoxazine is:
[0008] (1) adding 2-allylphenol and triethylamine to a toluene solvent, mixing them evenly, introducing nitrogen protection, and then adding phenylphosphonyl dichloride thereto, heating to 75-90° C. to react for 8-9 hours, washing with water, rotary distilling, standing overnight, and vacuum drying to obtain a diene phosphide;
[0009] (2) adding diene phosphide to N,N-dimethylformamide solvent, stirring and dispersing, adding L-cysteine and benzoin dimethyl ether photoinitiator, irradiating with 365 nm ultraviolet light at 25-40° C. for 3-5 h, centrifuging, washing and drying to obtain intermediate 1;
[0010] (3) Add 1-oxo-4-hydroxymethyl-1-phospha-2,6,7-trioxabicyclo[2.2.2]octane and intermediate 1 to ethyl acetate solvent, stir and dissolve, continue to add p-toluenesulfonic acid catalyst, heat to 75-100° C., stir and reflux for 12-16 hours, distill under reduced pressure after the reaction, wash with ether, and recrystallize the crude product with ethyl acetate to obtain intermediate 2;
[0011] (4) The intermediate 2, the aqueous solution of formaldehyde and phenol are added to a toluene solvent, fully dissolved, and subjected to a cyclization reaction at 60-90° C. for 10-15 h. After completion, the reaction is distilled under reduced pressure, washed with deionized water, and the crude product is recrystallized from dichloromethane to obtain a phosphorus-containing modified benzoxazine.
[0012] Preferably, the mass ratio of 2-allylphenol, triethylamine and phenylphosphonic acid dichloride in (1) is 1.2-1.6:0.02-0.03:1.
[0013] Preferably, the mass ratio of diene phosphide, L-cysteine and benzoin dimethyl ether photoinitiator in (2) is 1:1.4-1.8:0.02-0.03.
[0014] Preferably, in (3), the mass ratio of 1-oxo-4-hydroxymethyl-1-phospha-2,6,7-trioxabicyclo[2.2.2]octane, intermediate 1, and p-toluenesulfonic acid catalyst is 1:0.8-1.3:0.03-0.05.
[0015] Preferably, the mass ratio of the intermediate 2, the formaldehyde aqueous solution, and the phenol in (4) is 1:1.3-1.6:1.2-1.4.
[0016] Preferably, the preparation method of the modified graphene oxide is:
[0017] S1. Add 6-14 parts by weight of diene phosphide, 8-12 parts by weight of propenol, 7-15 parts by weight of allyl glycidyl ether to a toluene solvent, stir to dissolve, introduce nitrogen protection, continue to add 0.02-0.04 parts by weight of dibenzoyl peroxide initiator, reflux at 75-90 ° C for 4-6h, cool to room temperature after completion, wash, and obtain a hydroxylated polymer;
[0018] S2. 10-25 parts by weight of graphene oxide is ultrasonically dispersed in 50-70 parts by weight of thionyl chloride, and after being evenly dispersed, the mixture is reacted at 70-75° C. for 18-22 hours, and after the reaction, the mixture is filtered, washed, and dried to obtain graphene chloride;
[0019] S3. Add 5-10 parts by weight of chlorinated graphene and 4-8 parts by weight of hydroxylated polymer into N,N-dimethylformamide solvent, stir and disperse, continue to add 0.01-0.03 parts by weight of triethylamine catalyst, react at 90-110°C for 6-10h, and then distill under reduced pressure and wash to obtain modified graphene oxide.
[0020] Preferably, the preparation method of the low-voltage cable containing modified graphene oxide is: adding phosphorus-modified benzoxazine, modified graphene oxide, nano aluminum hydroxide, polyethylene, maleic anhydride grafted polyethylene, calcium carbonate, and antioxidant 1010 to an internal mixer, mixing at 140-160° C. for 10-15 minutes, and then hot-pressing the mixed material in a flat vulcanizer, and molding at a pressure of 8-12 MPa for 4-7 minutes to obtain a low-voltage cable containing modified graphene oxide.
[0021] (III) Beneficial technical effects
[0022] The present invention adds phosphorus-modified benzoxazine, modified graphene oxide, nano aluminum hydroxide, polyethylene, maleic anhydride grafted polyethylene, calcium carbonate, and antioxidant 1010 into an internal mixer, mixes them, and then hot-presses the mixed materials in a flat vulcanizer to obtain a low-voltage cable containing modified graphene oxide.
[0023] Phosphorus, sulfur and graphene oxide in phosphorus-modified benzoxazine and modified graphene oxide all have good flame retardant effects and together constitute a flame retardant system; and diene phosphide reacts with L-cysteine to increase the degree of sulfur substitution, further improving its flame retardant effect. The benzoxazine in phosphorus-modified benzoxazine will form a heat-resistant phenolic resin structure at high temperatures, making the cable show a higher thermal decomposition temperature and having a good flame retardant effect. At the same time, the phenolic hydroxyl group in the phenolic resin structure and the hydroxyl group in the modified graphene oxide will react with the anhydride group in the maleic anhydride grafted polyethylene to form a cross-linked network, making the connection more tightly and increasing the tensile properties between each other. DETAILED DESCRIPTION
[0024] Example 1
[0025] (1) adding 2-allylphenol and triethylamine to a toluene solvent, mixing them evenly, introducing nitrogen protection, and then adding phenylphosphonyl dichloride, wherein the mass ratio of 2-allylphenol, triethylamine and phenylphosphonyl dichloride is 1.2:0.02:1, heating to 75°C for 8 hours, washing with water after the reaction, rotary distillation, standing overnight, and vacuum drying to obtain a diene phosphide;
[0026] (2) adding diene phosphide to N,N-dimethylformamide solvent, stirring and dispersing, and then adding L-cysteine and benzoin dimethyl ether photoinitiator, wherein the mass ratio of diene phosphide, L-cysteine, and benzoin dimethyl ether photoinitiator is 1:1.4:0.02, irradiating with 365 nm ultraviolet light at 25° C. for 3 h, centrifuging after the end, washing and drying to obtain intermediate 1;
[0027] (3) adding 1-oxo-4-hydroxymethyl-1-phospha-2,6,7-trioxabicyclo[2.2.2]octane and intermediate 1 to ethyl acetate solvent, stirring to dissolve, and continuously adding p-toluenesulfonic acid catalyst thereto, wherein the mass ratio of 1-oxo-4-hydroxymethyl-1-phospha-2,6,7-trioxabicyclo[2.2.2]octane, intermediate 1, and p-toluenesulfonic acid catalyst is 1:0.8:0.03, heating to 75° C., stirring and reflux for 12 h, distilling under reduced pressure after the reaction, washing with ether, and recrystallizing the crude product from ethyl acetate to obtain intermediate 2;
[0028] (4) adding intermediate 2, an aqueous solution of formaldehyde, and phenol to a toluene solvent, wherein the mass ratio of intermediate 2, the aqueous solution of formaldehyde, and phenol is 1:1.3:1.2, fully dissolving, and carrying out a cyclization reaction at 60° C. for 10 h. After completion, distillation under reduced pressure is performed, the product is washed with deionized water, and the crude product is recrystallized from dichloromethane to obtain a phosphorus-modified benzoxazine;
[0029] (5) Add 6 parts by weight of diene phosphide, 8 parts by weight of allyl alcohol, and 7 parts by weight of allyl glycidyl ether to a toluene solvent, stir and dissolve, introduce nitrogen protection, continue to add 0.02 parts by weight of dibenzoyl peroxide initiator, reflux at 75° C. for 4 hours, cool to room temperature after completion, wash, and obtain a hydroxylated polymer;
[0030] (6) ultrasonically dispersing 10 parts by weight of graphene oxide into 50 parts by weight of thionyl chloride, and after being evenly dispersed, reacting at 70° C. for 18 hours, and after the reaction, filtering, washing, and drying to obtain chlorinated graphene;
[0031] (7) adding 5 parts by weight of chlorinated graphene and 4 parts by weight of hydroxylated polymer to N,N-dimethylformamide solvent, stirring and dispersing, adding 0.01 parts by weight of triethylamine catalyst thereto, reacting at 90° C. for 6 h, and then distilling under reduced pressure and washing to obtain modified graphene oxide;
[0032] (8) 4 parts by weight of phosphorus-modified benzoxazine, 3 parts by weight of modified graphene oxide, 1 part by weight of nano-aluminum hydroxide, 75 parts by weight of polyethylene, 40 parts by weight of maleic anhydride grafted polyethylene, 1 part by weight of calcium carbonate, and 0.2 parts by weight of antioxidant 1010 were added to an internal mixer and mixed at 140° C. for 10 min. The mixed material was then hot-pressed in a flat vulcanizer and molded at a pressure of 8 MPa for 4 min to obtain a low-voltage cable containing modified graphene oxide.
[0033] Example 2
[0034] (1) adding 2-allylphenol and triethylamine to a toluene solvent, mixing them evenly, introducing nitrogen protection, and then adding phenylphosphonyl dichloride, wherein the mass ratio of 2-allylphenol, triethylamine and phenylphosphonyl dichloride is 1.6:0.03:1, heating to 90° C. to react for 9 hours, washing with water after the reaction, rotary distilling, standing overnight, and vacuum drying to obtain a diene phosphide;
[0035] (2) adding diene phosphide to N,N-dimethylformamide solvent, stirring and dispersing, and then adding L-cysteine and benzoin dimethyl ether photoinitiator, wherein the mass ratio of diene phosphide, L-cysteine, and benzoin dimethyl ether photoinitiator is 1:1.8:0.03, irradiating with 365 nm ultraviolet light at 40° C. for 5 h, centrifuging after the end, washing and drying to obtain intermediate 1;
[0036] (3) adding 1-oxo-4-hydroxymethyl-1-phospha-2,6,7-trioxabicyclo[2.2.2]octane and intermediate 1 to ethyl acetate solvent, stirring to dissolve, and continuously adding p-toluenesulfonic acid catalyst thereto, wherein the mass ratio of 1-oxo-4-hydroxymethyl-1-phospha-2,6,7-trioxabicyclo[2.2.2]octane, intermediate 1, and p-toluenesulfonic acid catalyst is 1:1.3:0.03-0.05, heating to 100° C., stirring and reflux for 16 h, distilling under reduced pressure after the reaction, washing with ether, and recrystallizing the crude product from ethyl acetate to obtain intermediate 2;
[0037] (4) adding intermediate 2, an aqueous solution of formaldehyde, and phenol to a toluene solvent, wherein the mass ratio of intermediate 2, the aqueous solution of formaldehyde, and phenol is 1:1.6:1.2-1.4, fully dissolving, and carrying out a cyclization reaction at 90° C. for 15 h. After completion, distillation under reduced pressure is performed, and the crude product is washed with deionized water. Recrystallization of the dichloromethane is performed to obtain a phosphorus-containing modified benzoxazine;
[0038] (5) adding 14 parts by weight of diene phosphide, 12 parts by weight of allyl alcohol, and 15 parts by weight of allyl glycidyl ether to a toluene solvent, stirring to dissolve, introducing nitrogen protection, and continuing to add 0.04 parts by weight of dibenzoyl peroxide initiator, reflux at 90° C. for 6 hours, cooling to room temperature after completion, washing, and obtaining a hydroxylated polymer;
[0039] (6) ultrasonically dispersing 25 parts by weight of graphene oxide into 70 parts by weight of thionyl chloride, and after being evenly dispersed, reacting at 75° C. for 22 hours, and after the reaction, filtering, washing, and drying to obtain chlorinated graphene;
[0040] (7) adding 10 parts by weight of chlorinated graphene and 8 parts by weight of hydroxylated polymer to N,N-dimethylformamide solvent, stirring and dispersing, adding 0.03 parts by weight of triethylamine catalyst thereto, reacting at 110° C. for 10 h, and then distilling under reduced pressure and washing to obtain modified graphene oxide;
[0041] (8) 9 parts by weight of phosphorus-modified benzoxazine, 6 parts by weight of modified graphene oxide, 2 parts by weight of nano-aluminum hydroxide, 90 parts by weight of polyethylene, 60 parts by weight of maleic anhydride grafted polyethylene, 2 parts by weight of calcium carbonate, and 0.4 parts by weight of antioxidant 1010 were added to an internal mixer and mixed at 160° C. for 15 min. The mixed material was then hot-pressed in a flat vulcanizer and molded at a pressure of 12 MPa for 7 min to obtain a low-voltage cable containing modified graphene oxide.
[0042] Example 3
[0043] (1) adding 2-allylphenol and triethylamine to a toluene solvent, mixing well, introducing nitrogen protection, and then adding phenylphosphonyl dichloride, wherein the mass ratio of 2-allylphenol, triethylamine and phenylphosphonyl dichloride is 1.4:0.025:1, heating to 82° C. and reacting for 8.5 hours, washing with water after the reaction, rotary distilling, standing overnight, and vacuum drying to obtain a diene phosphide;
[0044] (2) adding diene phosphide to N,N-dimethylformamide solvent, stirring and dispersing, and then adding L-cysteine and benzoin dimethyl ether photoinitiator, wherein the mass ratio of diene phosphide, L-cysteine, and benzoin dimethyl ether photoinitiator is 1:1.6:0.025, irradiating with 365 nm ultraviolet light at 32° C. for 4 h, centrifuging after the end, washing and drying to obtain intermediate 1;
[0045] (3) Add 1-oxo-4-hydroxymethyl-1-phospha-2,6,7-trioxabicyclo[2.2.2]octane and intermediate 1 to ethyl acetate solvent, stir and dissolve, continue to add p-toluenesulfonic acid catalyst, wherein the mass ratio of 1-oxo-4-hydroxymethyl-1-phospha-2,6,7-trioxabicyclo[2.2.2]octane, intermediate 1 and p-toluenesulfonic acid catalyst is 1:1:0.04, heat to 87° C., stir and reflux for 14 hours, distill under reduced pressure after the reaction, wash with ether, and recrystallize the crude product with ethyl acetate to obtain intermediate 2;
[0046] (4) adding intermediate 2, an aqueous solution of formaldehyde, and phenol to a toluene solvent, wherein the mass ratio of intermediate 2, the aqueous solution of formaldehyde, and phenol is 1:1.4:1.3, fully dissolving, and carrying out a cyclization reaction at 75° C. for 12.5 h. After completion, distillation under reduced pressure is carried out, the product is washed with deionized water, and the crude product is recrystallized from dichloromethane to obtain a phosphorus-modified benzoxazine;
[0047] (5) adding 10 parts by weight of diene phosphide, 10 parts by weight of allyl alcohol, and 11 parts by weight of allyl glycidyl ether to a toluene solvent, stirring and dissolving, introducing nitrogen protection, and continuously adding 0.03 parts by weight of dibenzoyl peroxide initiator thereto, reflux reacting at 82° C. for 5 h, cooling to room temperature after completion, and washing to obtain a hydroxylated polymer;
[0048] (6) ultrasonically dispersing 17 parts by weight of graphene oxide into 60 parts by weight of thionyl chloride, and after being evenly dispersed, reacting at 72° C. for 20 h, and after the reaction, filtering, washing, and drying to obtain chlorinated graphene;
[0049] (7) adding 7.5 parts by weight of chlorinated graphene and 6 parts by weight of hydroxylated polymer to N,N-dimethylformamide solvent, stirring and dispersing, adding 0.02 parts by weight of triethylamine catalyst thereto, reacting at 100° C. for 8 h, and then performing reduced pressure distillation and washing to obtain modified graphene oxide;
[0050] (8) 6 parts by weight of phosphorus-modified benzoxazine, 4 parts by weight of modified graphene oxide, 1.5 parts by weight of nano-aluminum hydroxide, 82 parts by weight of polyethylene, 50 parts by weight of maleic anhydride grafted polyethylene, 1.5 parts by weight of calcium carbonate, and 0.3 parts by weight of antioxidant 1010 were added to an internal mixer and mixed at 150° C. for 12 min. The mixed material was then hot-pressed in a flat vulcanizer and molded at a pressure of 10 MPa for 5 min to obtain a low-voltage cable containing modified graphene oxide.
[0051] Comparative Example 1
[0052] 4 parts by weight of modified graphene oxide, 1.5 parts by weight of nano-aluminum hydroxide, 82 parts by weight of polyethylene, 50 parts by weight of maleic anhydride grafted polyethylene, 1.5 parts by weight of calcium carbonate, and 0.3 parts by weight of antioxidant 1010 were added to an internal mixer and mixed at 150° C. for 12 minutes. The mixed material was then hot-pressed in a flat vulcanizer and molded at a pressure of 10 MPa for 5 minutes to obtain a low-voltage cable containing modified graphene oxide.
[0053] Comparative Example 2
[0054] 6 parts by weight of phosphorus-modified benzoxazine, 1.5 parts by weight of nano-aluminum hydroxide, 82 parts by weight of polyethylene, 50 parts by weight of maleic anhydride grafted polyethylene, 1.5 parts by weight of calcium carbonate, and 0.3 parts by weight of antioxidant 1010 were added to an internal mixer and mixed at 150° C. for 12 minutes. The mixed material was then hot-pressed in a flat vulcanizer and molded at a pressure of 10 MPa for 5 minutes to obtain a low-voltage cable containing modified graphene oxide.
[0055] The limiting oxygen index of the low-voltage cable containing modified graphene oxide was tested using an oxygen index meter; the combustion level of the low-voltage cable containing modified graphene oxide was tested using a horizontal and vertical combustion instrument.
[0056] Table 1: Flame retardancy tests.
[0057] project Limiting oxygen index (%) Combustion level Example 1 31 V-0 Example 2 33 V-0 Example 3 32 V-0 Comparative Example 1 21 V-1 Comparative Example 2 22 V-1
[0058] It can be seen from Table 1 that Examples 1-3 have better flame retardant effects than Comparative Examples 1-2, indicating that the low-voltage cable containing modified graphene oxide prepared by the present invention has good flame retardant effects.
[0059] The tensile test was carried out in accordance with GB / T 1040.1-2018. The test results are shown in Table 2.
[0060] Table 2: Tensile strength test.
[0061]
[0062]
[0063] As can be seen from Table 2, low-voltage cable embodiments 1-3 containing modified graphene oxide of the present invention have better tensile properties than comparative examples 1-2.
[0064] The preferred embodiments of the present invention disclosed above are only used to help illustrate the present invention. The preferred embodiments do not describe all the details in detail, nor do they limit the invention to the specific implementation methods described. Obviously, many modifications and changes can be made according to the content of this specification. This specification selects and specifically describes these embodiments in order to better explain the principles and practical applications of the present invention, so that those skilled in the art can understand and use the present invention well. The present invention is limited only by the claims and their full scope and equivalents.
Claims
1. A low voltage cable containing modified graphene oxide, It is characterized in that The invention comprises the following components by weight: 4-9 parts by weight of phosphorus-modified benzoxazine, 3-6 parts by weight of modified graphene oxide, 1-2 parts by weight of nano aluminum hydroxide, 75-90 parts by weight of polyethylene, 40-60 parts by weight of maleic anhydride grafted polyethylene, 1-2 parts by weight of calcium carbonate and 0.2-0.4 parts by weight of antioxidant 1010.
2. The low-voltage cable containing modified graphene oxide according to claim 1, It is characterized in that The preparation method of the phosphorus-modified benzoxazine is as follows: (1) adding 2-allylphenol and triethylamine to a toluene solvent, mixing them evenly, introducing nitrogen protection, and then adding phenylphosphonyl dichloride thereto, heating to 75-90° C. to react for 8-9 hours, washing with water, rotary distilling, standing overnight, and vacuum drying to obtain a diene phosphide; (2) adding diene phosphide to N,N-dimethylformamide solvent, stirring and dispersing, adding L-cysteine and benzoin dimethyl ether photoinitiator, irradiating with 365 nm ultraviolet light at 25-40° C. for 3-5 h, centrifuging, washing and drying to obtain intermediate 1; (3) Add 1-oxo-4-hydroxymethyl-1-phospha-2,6,7-trioxabicyclo[2.2.2]octane and intermediate 1 to ethyl acetate solvent, stir and dissolve, continue to add p-toluenesulfonic acid catalyst, heat to 75-100° C., stir and reflux for 12-16 hours, distill under reduced pressure after the reaction, wash with ether, and recrystallize the crude product with ethyl acetate to obtain intermediate 2; (4) The intermediate 2, the aqueous solution of formaldehyde and phenol are added to a toluene solvent, fully dissolved, and subjected to a cyclization reaction at 60-90° C. for 10-15 h. After completion, the reaction is distilled under reduced pressure, washed with deionized water, and the crude product is recrystallized from dichloromethane to obtain a phosphorus-containing modified benzoxazine.
3. The low-voltage cable containing modified graphene oxide according to claim 2, It is characterized in that The mass ratio of 2-allylphenol, triethylamine and phenylphosphonic acid dichloride in (1) is 1.2-1.6:0.02-0.03:
1.
4. The low-voltage cable containing modified graphene oxide according to claim 2, It is characterized in that The mass ratio of diene phosphide, L-cysteine and benzoin dimethyl ether photoinitiator in (2) is 1:1.4-1.8:0.02-0.
03.
5. The low-voltage cable containing modified graphene oxide according to claim 2, It is characterized in that The mass ratio of 1-oxo-4-hydroxymethyl-1-phospha-2,6,7-trioxabicyclo[2.2.2]octane, intermediate 1 and p-toluenesulfonic acid catalyst in (3) is 1:0.8-1.3:0.03-0.
05.
6. The low-voltage cable containing modified graphene oxide according to claim 2, It is characterized in that The mass ratio of the intermediate 2, the aqueous solution of formaldehyde and the phenol in (4) is 1:1.3-1.6:1.2-1.
4.
7. The low-voltage cable containing modified graphene oxide according to claim 1, It is characterized in that The preparation method of the modified graphene oxide is: S1. Add 6-14 parts by weight of diene phosphide, 8-12 parts by weight of propenol, 7-15 parts by weight of allyl glycidyl ether to a toluene solvent, stir to dissolve, introduce nitrogen protection, continue to add 0.02-0.04 parts by weight of dibenzoyl peroxide initiator, reflux at 75-90 ° C for 4-6h, cool to room temperature after completion, wash, and obtain a hydroxylated polymer; S2. 10-25 parts by weight of graphene oxide is ultrasonically dispersed in 50-70 parts by weight of thionyl chloride, and after being evenly dispersed, the mixture is reacted at 70-75° C. for 18-22 hours, and after the reaction, the mixture is filtered, washed, and dried to obtain graphene chloride; S3. Add 5-10 parts by weight of chlorinated graphene and 4-8 parts by weight of hydroxylated polymer into N,N-dimethylformamide solvent, stir and disperse, continue to add 0.01-0.03 parts by weight of triethylamine catalyst, react at 90-110°C for 6-10h, and then distill under reduced pressure and wash to obtain modified graphene oxide.
8. A method for preparing a low-voltage cable containing modified graphene oxide according to any one of claims 1 to 7, It is characterized in that The preparation method of the low-voltage cable containing modified graphene oxide is as follows: phosphorus-modified benzoxazine, modified graphene oxide, nano aluminum hydroxide, polyethylene, maleic anhydride grafted polyethylene, calcium carbonate, and antioxidant 1010 are added to an internal mixer, mixed at 140-160° C. for 10-15 minutes, and then the mixed materials are hot-pressed in a flat vulcanizer, and molded at a pressure of 8-12 MPa for 4-7 minutes to obtain the low-voltage cable containing modified graphene oxide.