High-rate EVA (Ethylene Vinyl Acetate) composite anti-shrinkage elastomer and preparation method thereof
By introducing SEBS, modified kaolin, modified zinc oxide and other raw materials into EVA foaming materials, the problem of insufficient deformation and wear resistance of EVA foaming materials is solved, and the material's elasticity and wear resistance are improved. It is suitable for High-end shoe material production.
Patent Information
- Application Number
- CN202411381322.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-30
- Publication Date
- 2024-12-06
AI Technical Summary
EVA foaming materials have disadvantages such as large deformation, poor wear resistance, non-slip, and low-temperature hardening, which limits their wide application. Unhydrogenated modified SBS is susceptible to temperature and ultraviolet rays to cause oxidation and deterioration.
The formulation of EVA composite shrinkage-resistant elastomer includes EVA, SEBS, modified kaolin, modified zinc oxide and other raw materials. The dispersion and mechanical strength of the materials are improved by the preparation method of modified kaolin and zinc oxide, and combined with the elastic properties of SEBS , enhance the wear resistance and resilience of the material, and introduce antioxidants to improve stability.
It significantly improves the feel and texture, enhances the resilience, reduces the weight, improves the compression, provides anti-slip and wear resistance, extends the service life of the material, and is suitable for shoe material production.
Abstract
Description
Technical Field
[0001] The invention belongs to the field of EVA foaming, and in particular relates to a large-ratio EVA composite anti-shrinkage elastomer and a preparation method thereof. Background Art
[0002] Ethylene-vinyl acetate copolymer (EVA) is a thermoplastic resin with excellent flexibility, elasticity, stress crack resistance and good plastic processability.
[0003] Shoe materials made of EVA have the properties of light weight, softness, good elasticity, and shock absorption. In China, mid-to-high-end sports shoes, hiking shoes, slippers, sandals and other shoe materials industries are one of the main application areas of EVA. However, EVA foam materials have the disadvantages of large deformation, poor wear resistance, non-slip, and low-temperature hardening, which limits its wide application. Polystyrene-ethylene / butylene-styrene (SEBS) has low shrinkage, plasticity, high elasticity, easy processing, high strength and toughness, as well as excellent aging resistance and chemical stability. It can be used in various thermoplastic rubbers / plastics as impact-resistant, non-slip, wear-resistant, compression-resistant, and cold-resistant modified materials. Blending SEBS with EVA can significantly improve the viscoelasticity, wear resistance, and low-temperature hardening of EVA, so that the obtained shoe foam material takes into account the advantages of both.
[0004] Chinese patent CN 114989521 B discloses a heat shrinkage resistant and impact resistant foaming material and its preparation method and application. The raw materials of the foaming material include EVA, olefin block copolymer OBC, hollow microspheres, modified SBS, nano-silicon dioxide, crosslinking agent BIPB, zinc oxide and zinc stearate. The modified SBS is obtained by modifying the SBS material with expandable microspheres. The foaming material provided by this invention has excellent heat shrinkage resistance and impact resistance. However, the unhydrogenated modified SBS used in the foaming material raw material contains unsaturated carbon double bonds, which are more easily affected by temperature and ultraviolet rays, resulting in oxidation and deterioration.
[0005] Therefore, there is an urgent need for a large-ratio EVA composite anti-shrinkage elastomer that has anti-slip and wear-resistant properties and good resilience. Summary of the invention
[0006] In view of the existing technical problems, the purpose of the present invention is to provide a large-ratio EVA composite anti-shrinkage elastomer and a preparation method thereof. The EVA composite anti-shrinkage elastomer of the present invention improves the feel and texture, enhances the resilience, reduces the deadweight, improves the compression distortion, and has anti-slip and wear resistance, can be used to make shoe materials, and has high market value.
[0007] In order to achieve the above object, the technical solution adopted by the present invention is as follows:
[0008] On the one hand, the present invention provides a large-ratio EVA composite anti-shrinkage elastomer, which comprises the following raw materials in parts by weight: 40-60 parts of EVA, 10-25 parts of SEBS, 5-15 parts of SSBR, 10-15 parts of OBC, 4-8 parts of BIIR, 1-3 parts of modified kaolin, 2-3 parts of light calcium carbonate, 0.5-1.5 parts of a cross-linking agent, 2-3 parts of a high-temperature foaming agent, 1-2 parts of modified zinc oxide, 0.4-0.8 parts of stearic acid, 10-20 parts of cyclohexane oil, and 0.5-2 parts of an antioxidant.
[0009] Preferably, the VA content of the EVA is 15-35wt%.
[0010] The reaction mechanism and effects of the present invention are as follows:
[0011] 1. Kaolin is a clay or clay rock mainly composed of kaolinite minerals. Its layered structure and high hardness can improve the dimensional stability and wear resistance of EVA foaming materials; in addition, kaolin can improve the tolerance, fire resistance and heat resistance of EVA foaming materials to chemicals, and increase the service life of shoe materials. The present invention uses 2-(N-ethylperfluorooctanesulfonylamino)acetic acid and epichlorohydrin to synthesize a new type of fluorine-containing compound, and then obtains modified kaolin through ion exchange between kaolin layers, thereby improving its dispersibility in foaming materials.
[0012] On the one hand, the surface energy of fluorinated compounds is very low, which causes kaolin to migrate to the outer surface of the product during the foaming and curing process of EVA foam materials, resulting in a gradient distribution of kaolin content from the outer layer to the inner layer of the EVA foam product. In the outer layer of the product, the kaolin content is higher, which helps to improve the wear resistance of the EVA foam material; while the kaolin content in the inner layer is relatively low, which helps to improve the resilience of the EVA foam material.
[0013] On the other hand, the presence of epoxy groups on modified kaolin can improve the stability of EVA foamed shoe materials at high temperatures, reduce thermal decomposition, and enhance resistance to heat shrinkage; at the same time, epoxy groups can enhance the bonding performance of EVA foamed shoe materials with other materials (such as rubber, leather, etc.) and improve the overall durability of the shoe materials; in addition, epoxy groups may form chemical crosslinks with other functional groups in the foaming material to improve the mechanical strength and heat resistance of the material.
[0014] 2. One of the main functions of zinc oxide in the production process of shoe materials is to promote foaming. As an important inorganic foaming accelerator, zinc oxide plays a particularly important role in foamed products using EVA as raw materials. Zinc oxide can reduce the decomposition temperature of the foaming agent, facilitate production, improve the production efficiency of EVA foamed shoe materials, and maintain the stability of the product. However, zinc oxide has poor dispersibility in the polymer system and cannot play its role well.
[0015] The present application uses silane coupling agent KH-570 to modify zinc oxide. The ethoxy group at one end of the silane coupling agent undergoes a coupling reaction with zinc oxide and is grafted onto the surface of zinc oxide to improve its dispersibility in the polymer matrix. The uniformity of dispersion can not only more effectively catalyze the decomposition of the foaming agent, and the decomposition products are transferred to nitrogen, carbon dioxide and ammonia, the formamide content will be reduced, but also the mechanical strength of the EVA foaming material can be improved.
[0016] Furthermore, the applicant grafted N,N'-methylenebisacrylamide through unsaturated double bonds. On the one hand, the introduced amino group has a similar polarity to the amino group on the foaming agent, so the modified zinc oxide has good compatibility with the foaming agent, effectively and evenly catalyzes the decomposition of the foaming agent, and controls the uniformity of foaming; on the other hand, the double bonds of N,N'-methylenebisacrylamide will cross-link with EVA and SEBS, enhancing the mechanical properties and heat resistance of the material and improving its resistance to thermal shrinkage.
[0017] 3. SEBS elastomer is light, soft and has good stretchability. Using SEBS elastomer together with EVA and other auxiliary materials can effectively increase the foaming efficiency of the material during the foaming process, shorten the foaming time, and effectively improve the elasticity of the EVA material, reduce the weight of the foamed sole, improve compression distortion, and at the same time improve the strong plastic feel caused by EVA foaming, and improve the feel and texture.
[0018] In some embodiments, the method for preparing the modified kaolin comprises the following steps:
[0019] (1) adding 2-(N-ethylperfluorooctanesulfonylamino)acetic acid and N,N-dimethylformamide to a reaction kettle, stirring for 30-60 minutes, adding epichlorohydrin, heating to 90-105° C., and rotary evaporating to obtain a fluorine-containing compound;
[0020] (2) Add kaolin to deionized water, stir for 30-60 minutes, age for 16-24 hours, heat to 75-85° C., add the fluorine-containing compound obtained in step (1), ultrasonically treat for 15-30 minutes, keep warm for reaction for 3-4 hours, cool, centrifuge, wash, dry, grind and sieve to obtain modified kaolin.
[0021] In some embodiments, the mass ratio of 2-(N-ethylperfluorooctanesulfonylamino)acetic acid to epichlorohydrin in step (1) is 1:(0.16-0.22).
[0022] In some embodiments, the mass ratio of kaolin and fluorine-containing compound in step (2) is (2-5):1.
[0023] In some embodiments, the method for preparing the modified zinc oxide comprises the following steps:
[0024] S1. Add zinc oxide, anhydrous ethanol and deionized water to a reactor, ultrasonically treat for 10-30 minutes, heat to 75-85°C, dropwise add silane coupling agent KH-570, ultrasonically treat for 30-45 minutes, cool to room temperature, wash, centrifuge, and dry to obtain a modified intermediate;
[0025] S2. The modified intermediate obtained in step S1 is mixed with N,N'-methylenebisacrylamide, and ball-milled for 1-2 hours to obtain modified zinc oxide.
[0026] In some embodiments, the mass ratio of zinc oxide to silane coupling agent KH-570 in step S1 is 1:(1.05-1.3).
[0027] In some embodiments, the mass ratio of the modified intermediate and N,N'-methylenebisacrylamide in step S2 is (2-3.5):1.
[0028] Preferably, the zinc oxide is nano zinc oxide.
[0029] In some embodiments, the cross-linking agent is dicumyl peroxide and / or 1,4-di-tert-butylperoxycumene.
[0030] In some embodiments, the high temperature foaming agent is azodicarbonamide and / or N,N'-dinitrosopentamethylenetetramine.
[0031] Preferably, the blowing agent is azodicarbonamide.
[0032] More preferably, the foaming agent is azodicarbonamide AC-3500.
[0033] Another aspect of the present invention provides a method for preparing a large-ratio EVA composite anti-shrinkage elastomer, comprising the following steps:
[0034] 1. Add SEBS, SSBR, OBC, BIIR, modified kaolin, light calcium carbonate, stearic acid, cyclohexane oil and antioxidant into a twin-screw extruder for extrusion granulation to obtain a modified elastomer;
[0035] 2. The modified elastomer obtained in step 1, EVA, a cross-linking agent, a high-temperature foaming agent, and modified zinc oxide are mixed and then internally kneaded, and then open-mixed and granulated to obtain the EVA composite anti-shrinkage elastomer.
[0036] Compared with the prior art, the present invention has the following beneficial effects:
[0037] 1. The EVA composite anti-shrinkage elastomer prepared by the present invention improves the feel and texture, enhances the resilience, reduces the dead weight, improves the compression distortion, and has anti-slip and wear resistance, can be used to make shoe materials, and has high market value.
[0038] 2. The modified kaolin of the present invention has excellent dispersion performance in the foaming material, which improves the wear resistance and resilience of the EVA foaming material; at the same time, the modified kaolin can improve the stability of the EVA foaming shoe material at high temperature, enhance the heat shrinkage resistance, and enhance the bonding performance of the EVA foaming shoe material with other materials (such as rubber, leather, etc.).
[0039] 3. The modified zinc oxide of the present invention has good dispersibility in the foaming material, which can not only more effectively catalyze the decomposition of the foaming agent, but also improve the mechanical strength of the EVA foaming material. Furthermore, the applicant introduced N,N'-methylenebisacrylamide. On the one hand, the introduced amino group increases the compatibility, effectively and evenly catalyzes the decomposition of the foaming agent, and controls the uniformity of foaming; on the other hand, the double bonds of N,N'-methylenebisacrylamide will cross-link with EVA and SEBS, enhance the mechanical properties and heat resistance of the material, and improve the heat shrinkage resistance.
[0040] 4. The present invention uses SEBS elastomer together with EVA and other auxiliary materials, which can effectively increase the foaming efficiency of the material during the foaming process, shorten the foaming time, and effectively improve the elasticity of the EVA material, reduce the dead weight of the foamed sole, improve compression distortion, and at the same time improve the problem of strong plastic feel caused by EVA foaming, thereby improving the feel and texture. DETAILED DESCRIPTION
[0041] The present invention will be described below in conjunction with specific embodiments. It should be noted that the following embodiments are examples of the present invention and are only used to illustrate the present invention, rather than to limit the present invention. Other combinations and various modifications within the concept of the present invention may be performed without departing from the spirit or scope of the present invention.
[0042] According to the ratio of each raw material and the preparation method specified in the following examples and comparative examples, an EVA composite anti-shrinkage elastomer was prepared.
[0043] In order to facilitate those skilled in the art to implement the present invention, some raw material manufacturers of the embodiments and comparative examples are described as follows:
[0044] The uniform particle size of nano zinc oxide is 100nm;
[0045] Azodicarbonamide AC-3500: purchased from Dongguan Xinrun Trading Co., Ltd.;
[0046] Naphthenic oil N4010: purchased from Shandong Zhuyou Lubrication Technology Co., Ltd.;
[0047] EVA: purchased from Shanghai Yesu International Trading Co., Ltd., VA content 18wt%, model UE629;
[0048] OBC: purchased from Dongguan Xinrui New Materials Co., Ltd., Dow OBC, model XH4021CFMBMT;
[0049] Other raw materials are not specially specified and can be purchased from the market.
[0050] Preparation Example 1
[0051] The preparation method of modified kaolin A comprises the following steps:
[0052] (1) Add 10 g of 2-(N-ethylperfluorooctanesulfonylamino)acetic acid and 5000 ml of N,N-dimethylformamide to a reaction kettle, stir for 45 min, add 2 g of epichlorohydrin, heat to 95° C., and rotary evaporate to obtain a fluorine-containing compound;
[0053] (2) Add 28 g of kaolin to 280 ml of deionized water, stir for 45 min, age for 20 h, heat to 80° C., add 8 g of the fluorine-containing compound obtained in step (1), ultrasonically treat for 20 min, keep warm for 3.5 h, cool to room temperature, centrifuge, wash three times with deionized water, dry at 85° C. for 6 h, and grind through a 200-mesh sieve to obtain modified kaolin A.
[0054] Preparation Example 2
[0055] The preparation method of modified kaolin B is the same as that of Preparation Example 1, except that the amount of epichlorohydrin added in step (1) is 1.4 g.
[0056] Preparation Example 3
[0057] The preparation method of modified kaolin C is the same as that of Preparation Example 1, except that the amount of fluorine-containing compound added in step (2) is 15.5 g.
[0058] Preparation Example 4
[0059] The preparation method of modified zinc oxide A comprises the following steps:
[0060] S1. 5 g of nano zinc oxide, 200 ml of anhydrous ethanol and 300 ml of deionized water were added to a reactor, ultrasonically treated for 20 min, heated to 80 ° C, 6 g of silane coupling agent KH-570 was added dropwise, ultrasonically treated for 40 min, cooled to room temperature, washed with anhydrous ethanol 3 times, centrifuged, and dried at 60 ° C for 4 h to obtain a modified intermediate;
[0061] S2. 5.5 g of the modified intermediate obtained in step S1 and 2 g of N,N'-methylenebisacrylamide were mixed and ball-milled for 1.5 h to obtain modified zinc oxide.
[0062] Preparation Example 5
[0063] The preparation method of modified zinc oxide B is the same as that of Preparation Example 4, except that the amount of silane coupling agent KH-570 added in step S1 is 4.25 g.
[0064] Preparation Example 6
[0065] The preparation method of modified zinc oxide C is the same as that of Preparation Example 4, except that the amount of N,N'-methylenebisacrylamide added in step S2 is 1.45 g.
[0066] Example 1
[0067] A large-ratio EVA composite anti-shrinkage elastomer comprises the following raw materials, measured by weight: 50 parts of EVA, 18 parts of SEBS, 10 parts of SSBR, 12.5 parts of OBC, 6 parts of BIIR, 2 parts of modified kaolin A, 2.5 parts of light calcium carbonate, 1 part of dicumyl peroxide, 2.5 parts of azodicarbonamide AC-3500, 1.5 parts of modified zinc oxide A, 0.6 parts of stearic acid, 1015 parts of cyclohexane oil N40, and 1.5 parts of antioxidant 1010.
[0068] The preparation method of the EVA composite anti-shrinkage elastomer of the present embodiment comprises the following steps:
[0069] 1. Add SEBS, SSBR, OBC, BIIR, modified kaolin A, light calcium carbonate, stearic acid, naphthenic oil N4010 and antioxidant 1010 into a twin-screw extruder, adjust the screw speed to 20r / s, the temperature of each section of the screw to 160℃-180℃-190℃-200℃-200℃-200℃-190℃-190℃-180℃-170℃, and extrude and granulate to obtain a modified elastomer;
[0070] 2. The modified elastomer obtained in step 1, EVA, dicumyl peroxide, azodicarbonamide AC-3500 and modified zinc oxide A are mixed and then kneaded. The kneading temperature is adjusted to 120° C. and maintained for 20 minutes. Then, the mixture is open-mixed and granulated to obtain the EVA composite anti-shrinkage elastomer.
[0071] Example 2
[0072] A large-ratio EVA composite anti-shrinkage elastomer comprises the following raw materials in parts by weight: 40 parts of EVA, 10 parts of SEBS, 5 parts of SSBR, 10 parts of OBC, 4 parts of BIIR, 1 part of modified kaolin A, 2 parts of light calcium carbonate, 0.5 parts of dicumyl peroxide, 2 parts of azodicarbonamide AC-3500, 1 part of modified zinc oxide A, 0.4 parts of stearic acid, 10 parts of cyclohexane oil N4010, and 0.5 parts of antioxidant 1010.
[0073] The preparation method of the EVA composite anti-shrinkage elastomer in this embodiment is the same as that in Example 1.
[0074] Example 3
[0075] A large-ratio EVA composite anti-shrinkage elastomer comprises the following raw materials in parts by weight: 60 parts of EVA, 25 parts of SEBS, 15 parts of SSBR, 15 parts of OBC, 8 parts of BIIR, 3 parts of modified kaolin A, 3 parts of light calcium carbonate, 1.5 parts of dicumyl peroxide, 3 parts of azodicarbonamide AC-3500, 2 parts of modified zinc oxide A, 0.8 parts of stearic acid, 1020 parts of cyclohexane oil N40, and 10102 parts of antioxidant.
[0076] The preparation method of the EVA composite anti-shrinkage elastomer in this embodiment is the same as that in Example 1.
[0077] Example 4
[0078] A large-ratio EVA composite anti-shrinkage elastomer and a preparation method thereof, the specific implementation manner is the same as that of Example 1, except that an equal amount of modified kaolin B is used to replace modified kaolin A.
[0079] Example 5
[0080] A large-ratio EVA composite anti-shrinkage elastomer and a preparation method thereof, the specific implementation manner is the same as that of Example 1, except that an equal amount of modified kaolin C is used to replace modified kaolin A.
[0081] Example 6
[0082] A large-ratio EVA composite anti-shrinkage elastomer and a preparation method thereof, the specific implementation manner is the same as that of Example 1, except that an equal amount of modified zinc oxide B is used to replace modified zinc oxide A.
[0083] Example 7
[0084] A large-ratio EVA composite anti-shrinkage elastomer and a preparation method thereof, the specific implementation manner is the same as that of Example 1, except that an equal amount of modified zinc oxide C is used to replace modified zinc oxide A.
[0085] Comparative Example 1
[0086] A large-ratio EVA composite anti-shrinkage elastomer and a preparation method thereof, the specific implementation method is the same as that of Example 1, except that an equal amount of kaolin is used to replace modified kaolin A.
[0087] Comparative Example 2
[0088] A large-ratio EVA composite anti-shrinkage elastomer and a preparation method thereof, the specific implementation manner is the same as that of Example 1, except that an equal amount of nano zinc oxide is used to replace modified zinc oxide A.
[0089] Effect evaluation:
[0090] The EVA composite anti-shrinkage elastomers prepared in the above Examples 1-7 and Comparative Examples 1-2 were tested and analyzed, and the specific results are shown in Table 1.
[0091] Performance Testing:
[0092] (1) Thermal shrinkage test: in accordance with standard HG / T 2874-1997;
[0093] (2) Resilience test: according to ASTM D2632-01;
[0094] (3) Wear resistance test: in accordance with standard GB / T 3903.2-2008.
[0095] Table 1
[0096] Serial number Thermal shrinkage / % Resilience / % Wear resistance(mm) Example 1 1.5 56 7.8 Example 2 1.9 52 8.2 Example 3 1.7 54 8.0 Example 4 2.2 51 8.9 Example 5 2.0 44 7.5 Example 6 2.9 48 8.4 Example 7 3.1 50 8.2 Comparative Example 1 3.4 48 8.8 Comparative Example 2 3.6 42 9.5
[0097] From the results in Table 1, it can be seen that the EVA composite anti-shrinkage elastomers prepared in Examples 1-3 have low thermal shrinkage, good resilience and good wear resistance.
[0098] Compared with Example 1, when preparing modified kaolin, the mass ratio of 2-(N-ethylperfluorooctanesulfonylamino)acetic acid and epichlorohydrin was changed, the heat resistance decreased, and the heat shrinkage rate increased, which in turn affected the resilience and wear resistance.
[0099] Compared with Example 1, in Example 5, the mass ratio of kaolin and fluorine-containing compound is changed when preparing modified kaolin, and kaolin will migrate excessively to the outer surface of the product. Although the wear resistance is improved, the resilience is greatly reduced.
[0100] Compared with Example 1, when preparing modified zinc oxide, Example 6 changes the mass ratio of zinc oxide to silane coupling agent KH-570, so that the dispersibility of zinc oxide deteriorates, which in turn causes incomplete decomposition of the foaming agent and affects the overall performance of the EVA composite anti-shrinkage elastomer.
[0101] Compared with Example 1, when preparing modified zinc oxide, Example 7 changes the mass ratio of the modified intermediate and N,N'-methylenebisacrylamide, which affects the decomposition of the foaming agent, weakens the cross-linking effect, and reduces the heat resistance.
[0102] Compared with Example 1, Comparative Example 1 uses an equal amount of commercially available kaolin to replace modified kaolin A. The kaolin cannot migrate well during the foaming process, affecting the overall performance of the EVA composite anti-shrinkage elastomer.
[0103] Compared with Example 1, Comparative Example 2 uses an equal amount of commercially available zinc oxide to replace modified zinc oxide A. The zinc oxide has poor dispersibility, which reduces the overall performance of the EVA composite anti-shrinkage elastomer.
[0104] The above is only a preferred embodiment of the present invention and does not constitute any form of limitation to the present application. Although the present application is disclosed as above in the preferred embodiment, it is not intended to limit the present application. Any technician familiar with the profession, without departing from the scope of the technical solution of the present application, using the technical content disclosed above to make slight changes or modifications are equivalent to equivalent implementation cases. However, any simple modifications, equivalent changes and modifications made to the above embodiments based on the technical essence of the present invention without departing from the content of the technical solution of the present invention are still within the scope of the technical solution.
Claims
1. A high-ratio EVA composite anti-shrinkage elastomer, characterized in that: The invention comprises the following raw materials by weight: 40-60 parts of EVA, 10-25 parts of SEBS, 5-15 parts of SSBR, 10-15 parts of OBC, 4-8 parts of BIIR, 1-3 parts of modified kaolin, 2-3 parts of light calcium carbonate, 0.5-1.5 parts of crosslinking agent, 2-3 parts of high-temperature foaming agent, 1-2 parts of modified zinc oxide, 0.4-0.8 parts of stearic acid, 10-20 parts of cyclohexane oil and 0.5-2 parts of antioxidant.
2. The large-ratio EVA composite anti-shrinkage elastomer according to claim 1, characterized in that: The preparation method of the modified kaolin comprises the following steps: (1) adding 2-(N-ethylperfluorooctanesulfonylamino)acetic acid and N,N-dimethylformamide to a reaction kettle, stirring for 30-60 minutes, adding epichlorohydrin, heating to 90-105° C., and rotary evaporating to obtain a fluorine-containing compound; (2) Add kaolin to deionized water, stir for 30-60 minutes, age for 16-24 hours, heat to 75-85° C., add the fluorine-containing compound obtained in step (1), ultrasonically treat for 15-30 minutes, keep warm for reaction for 3-4 hours, cool, centrifuge, wash, dry, grind and sieve to obtain modified kaolin.
3. The large-ratio EVA composite anti-shrinkage elastomer according to claim 2, characterized in that: The mass ratio of 2-(N-ethylperfluorooctanesulfonylamino)acetic acid to epichlorohydrin in step (1) is 1:(0.16-0.22).
4. The large-ratio EVA composite anti-shrinkage elastomer according to claim 2, characterized in that: The mass ratio of kaolin and fluorine-containing compound in step (2) is (2-5):
1.
5. The large-ratio EVA composite anti-shrinkage elastomer according to claim 1, characterized in that: The preparation method of the modified zinc oxide comprises the following steps: S1. Add zinc oxide, anhydrous ethanol and deionized water to a reactor, ultrasonically treat for 10-30 minutes, heat to 75-85°C, dropwise add silane coupling agent KH-570, ultrasonically treat for 30-45 minutes, cool to room temperature, wash, centrifuge, and dry to obtain a modified intermediate; S2. The modified intermediate obtained in step S1 is mixed with N,N'-methylenebisacrylamide, and ball-milled for 1-2 hours to obtain modified zinc oxide.
6. The large-ratio EVA composite anti-shrinkage elastomer according to claim 5, characterized in that: The mass ratio of zinc oxide to silane coupling agent KH-570 in step S1 is 1:(1.05-1.3).
7. The large-ratio EVA composite anti-shrinkage elastomer according to claim 5, characterized in that: The mass ratio of the modified intermediate and N,N'-methylenebisacrylamide in step S2 is (2-3.5):
1.
8. The large-ratio EVA composite anti-shrinkage elastomer according to claim 1, characterized in that: The cross-linking agent is dicumyl peroxide and / or 1,4-di-tert-butyl peroxycumene.
9. The large-ratio EVA composite anti-shrinkage elastomer according to claim 1, characterized in that: The high temperature foaming agent is azodicarbonamide and / or N,N'-dinitrosopentamethylenetetramine.
10. A method for preparing the large-ratio EVA composite anti-shrinkage elastomer according to any one of claims 1 to 9, characterized in that: The following steps are included:
1. Add SEBS, SSBR, OBC, BIIR, modified kaolin, light calcium carbonate, stearic acid, cyclohexane oil and antioxidant into a twin-screw extruder for extrusion granulation to obtain a modified elastomer; 2. The modified elastomer obtained in step 1, EVA, a cross-linking agent, a high-temperature foaming agent, and modified zinc oxide are mixed and then internally kneaded, and then open-mixed and granulated to obtain the EVA composite anti-shrinkage elastomer.
Citation Information
Patent Citations
A kind of heat shrinkage resistant and impact resistant foaming material and its preparation method and application