High-molecular functional material with cell adhesion and preparation method thereof
Through the blending and melt blending technology of polydimethylammonium methacrylate and polypropylene, polymer materials with cell adhesion were prepared, which solved the problems of high cost of cell culture dishes and complex process in the prior art. It achieves efficient cell adhesion improvement and excellent cell culture ability.
Patent Information
- Application Number
- CN202411583184.9
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-11-07
- Publication Date
- 2024-12-06
- Estimated Expiration
- Not applicable · inactive patent
AI Technical Summary
Existing cell culture dishes have high cost and complex processes in improving cell adhesion, and a simple and efficient method is needed to prepare materials with cell adhesion.
By blending polydimethylammonium methacrylate with polypropylene and melt blending and stretching under specific conditions, polymer functional materials with cell adhesion were prepared for the preparation of coatings without requiring any coating cell culture dish.
It has achieved efficient and low cost improvement in cell adhesion, significantly improved cell density, and is better than the cell culture capability of commercial culture plates.
Smart Images

Figure CN119081295A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of functional polymer materials, and in particular relates to a preparation method of a polymer material with cell adhesion and an application of the polymer material in cell culture. Background Art
[0002] With the development of science and technology, cell engineering has been gradually applied to the fields of medicine, biotechnology and pharmaceuticals. Cell culture is the basis of cell engineering and molecular biology, providing an excellent model system for the study of normal cell physiology and biochemistry, and the effects of drugs and toxic compounds on cells. Cell culture can also be used for drug screening and development, as well as large-scale production of vaccines and therapeutic proteins.
[0003] The culture dishes used for cell culture are basic equipment in scientific experiments and are widely used in biomedicine and other fields. For cell culture, on the one hand, it is necessary to consider the operability of cell culture, and more importantly, how the cells adsorb and adhere to the material and grow healthily, while at the same time ensuring its safety and the rationality of actual production. At present, the raw materials of cell culture dish products are roughly divided into two categories: glass and plastic. Among them, the plastic component is generally polystyrene. However, in order for cells to maintain consistent cell growth in the culture dish, a layer of highly hydrophilic film must be coated on its surface to enhance the adhesion of the cells.
[0004] The prior art discloses a cell culture dish that can promote cell proliferation. The polysaccharide coating mainly composed of chondroitin sulfate can significantly increase the proliferation rate of chondrocytes in the culture dish. The above process is relatively complicated and the cost is also high. Based on this, it is urgent to develop a raw material for a new type of cell culture dish to prepare a culture dish with cell adhesion. Summary of the invention
[0005] The purpose of the present invention is to provide a polymer functional material with cell adhesion, and also to provide a preparation method and application of the polymer functional material with cell adhesion, so as to solve the problem of making the molecular functional material have good adhesion and preparing a culture dish with cell adhesion without coating.
[0006] The objective of the present invention is achieved through the following technical solutions: A method for preparing a polymer functional material with cell adhesion comprises the following steps: A. Preparation of polydimethylaminoethyl methacrylate: A1. Filter and purify dimethylaminoethyl methacrylate using a neutral alumina column to remove the polymerization inhibitor in its industrial product; A2, adding purified dimethylaminoethyl methacrylate monomer and initiator azobisisobutyronitrile into a reaction vessel, dissolving them in an organic solvent, and heating and stirring to react; A3, after the reaction is completed, place in a dialysis bag for 120 h, freeze-dry, and obtain poly (dimethylaminoethyl methacrylate); B. Preparation of polymer functional materials with cell adhesion by melt blending: B1, fully mixing polypropylene and the prepared polydimethylaminoethyl methacrylate according to a mass ratio, drying and grinding into powder to obtain a blend; B2, adding the blend into a twin-screw extruder, melt blending at 170-240° C., 160-300 r / min, and extruding granulation; B3. The product obtained in step B2 is sequentially stretched and heat-set to obtain a culture dish with cell adhesion.
[0007] Furthermore, in step A2, the amount of the initiator azobisisobutyronitrile is 0.04%-0.2%, the reaction time is 5-96 h, and the reaction temperature is 40-85°C.
[0008] Furthermore, the dosage of the azobisisobutyronitrile is 0.1%.
[0009] Furthermore, the reaction time is 24 hours and the reaction temperature is 70°C.
[0010] Furthermore, in step A2, the organic solvent is one or more of dimethyl sulfoxide, N,N-dimethylformamide, toluene and tetrahydrofuran.
[0011] Furthermore, the organic solvent is dimethyl sulfoxide.
[0012] Furthermore, in step A3, the dialysis freeze-drying process uses a dialysis bag with a molecular weight cut-off of 500-50000 Da.
[0013] Furthermore, in step B3, the preheating temperature for stretching is 100-150°C, the stretching temperature is 120-160°C, the stretching multiple is 4-6 times, and the setting temperature is 230-245°C.
[0014] A polymer functional material with cell adhesion is prepared by the above preparation method, and is composed of the following raw materials by mass percentage: polypropylene: 70-95%, poly(dimethylaminoethyl methacrylate): 5-30%; wherein the polypropylene is at least one of homopolymer polypropylene and copolymer polypropylene.
[0015] The invention discloses an application of a macromolecular functional material with cell adhesion, which can be used for cell culture. The macromolecular functional material with cell adhesion is melted by heating, and the melt passes through a die head to form a culture dish shape under the action of the die, and is cooled and shaped to obtain a culture dish with cell adhesion.
[0016] Compared with the prior art, the present invention has the following beneficial effects: The present invention provides a high molecular functional material with good cell adhesion, which comprises the following components by mass percentage: polypropylene (PP): 70-95%, poly(dimethylaminoethyl methacrylate) (PDM): 5-30%; since the amine group on the side chain of PDM can provide an effective adsorption site, the present invention introduces poly(dimethylaminoethyl methacrylate) to improve the adhesion performance of polypropylene materials to cells. Starting from the origin of culture dish preparation, the present invention prepares a new type of culture dish with strong cell adhesion by doping cationic polymers in the raw materials without subsequent surface modification, and the preparation process is simple, efficient and low-cost. Compared with commercial culture plates, the composite material of the present invention has a more excellent cell culture ability, and the cell density is significantly higher than that of commercial culture plates. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the drawings required for use in the embodiments are briefly introduced below. It should be understood that the following drawings only show certain embodiments of the present invention and therefore should not be regarded as limiting the scope. For ordinary technicians in this field, other related drawings can be obtained based on these drawings without creative work.
[0018] Figure 1 This is the NMR image of polydimethylaminoethyl methacrylate prepared in Example 1.
[0019] Figure 2 This is the GPC of polydimethylaminoethyl methacrylate prepared in Example 1.
[0020] Figure 3 Fluorescence microscope images of MCF7-GFP cell proliferation.
[0021] Figure 4 Technical roadmap for the preparation of dimethylaminoethyl methacrylate. DETAILED DESCRIPTION
[0022] The present invention will be further described below in conjunction with embodiments: The present invention will be further described in detail below in conjunction with the accompanying drawings and embodiments. It is to be understood that the specific embodiments described herein are only used to explain the present invention, rather than to limit the present invention. It should also be noted that, for ease of description, only parts related to the present invention, rather than all structures, are shown in the accompanying drawings.
[0023] It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once an item is defined in one drawing, it does not need to be further defined and explained in the subsequent drawings. At the same time, in the description of the present invention, the terms "first", "second", etc. are only used to distinguish the description and cannot be understood as indicating or implying relative importance.
[0024] The cell-adhesive macromolecular functional material of the present invention is composed of the following raw materials by mass percentage: 70-95% of polypropylene (PP) and 5-30% of polydimethylaminoethyl methacrylate (PDM).
[0025] Wherein, the polypropylene is at least one of homopolymer polypropylene and copolymer polypropylene.
[0026] The method for preparing the cell-adhesive polymer functional material of the present invention comprises the following steps: 1. Preparation of poly(dimethylaminoethyl methacrylate): 11. Filter and purify dimethylaminoethyl methacrylate using a neutral alumina column to remove the polymerization inhibitor in its industrial product; 12. Add purified dimethylaminoethyl methacrylate monomer and initiator azobisisobutyronitrile (AIBN) into a reaction vessel, dissolve in an organic solvent, and heat and stir to react; 13. After the reaction is completed, place it in a dialysis bag for 120 hours and freeze-dry to obtain poly (dimethylaminoethyl methacrylate).
[0027] Specifically, in step 12, the amount of the initiator azobisisobutyronitrile (AIBN) is 0.04%-0.2%, the reaction time is 5-96 h, and the reaction temperature is 40-85°C.
[0028] Preferably, the dosage of AIBN is 0.1%, the reaction time is 24h, and the reaction temperature is 70°C.
[0029] In step 12, the organic solvent is one or more of dimethyl sulfoxide, N,N-dimethylformamide, toluene and tetrahydrofuran.
[0030] Preferably, the organic solvent is dimethyl sulfoxide.
[0031] In step 13, the dialysis freeze-drying process uses a dialysis bag with a molecular weight cut-off of 500-50000 Da.
[0032] 2. Preparation of polymer functional materials with cell adhesion by melt blending: 21. Fully mix the polypropylene and the prepared poly(dimethylaminoethyl methacrylate) in a mass ratio, dry and grind into powder to obtain a blend; 22. Add the blend into a twin-screw extruder, melt blend at 170-240°C and 160-300 r / min, and extrude into granules; 23. The product of step B2 is sequentially stretched and heat-set to obtain a culture dish with cell adhesion.
[0033] Specifically, the preheating temperature for stretching in step 23 is 100-150°C, the stretching temperature is 120-160°C, the stretching ratio is 4-6 times, and the setting temperature is 230-245°C. Preferably, the preheating temperature is 110°C, the stretching temperature is 125°C, the stretching ratio is 4.5 times, and the setting temperature is 240°C.
[0034] The cell-adhesive polymer functional material prepared by the present invention can be used for cell culture. The prepared cell-adhesive polymer functional material is melted by heating, the melt passes through a die head, and is formed into a culture dish shape under the action of the mold, and is cooled and shaped to obtain a culture dish with cell adhesion.
[0035] The raw materials used in the following examples of the present invention are all commercially available products, all purchased from Aladdin Reagent.
[0036] like Figure 1 As shown, the signal peak at the chemical shift of 2.25-2.35ppm is the characteristic absorption peak of -NCH3 on the PDM chain, 2.65ppm is attributed to the characteristic absorption peak of -NCH2- on the PDM chain, and 4.09ppm is attributed to the proton characteristic absorption peak of -OCH2-. Figure 2 As shown, the GPC curves of polymer PDM are all symmetrical single peaks and have a narrow molecular weight distribution.
[0037] Example 1: Purified dimethylaminoethyl methacrylate (50 g) was placed in a 250 mL reaction bottle, DMSO was added to dissolve, and initiator AIBN (0.06 g) was added. Under nitrogen conditions, the reaction bottle was placed in a 70 ° C oil bath and stirred for reaction for 24 hours. After the reaction was completed, it was placed in a dialysis bag for dialyzation for 3 days and then freeze-dried to obtain polydimethylaminoethyl methacrylate PDM1.
[0038] Example 2: Purified dimethylaminoethyl methacrylate (50 g) was placed in a 250 mL reaction bottle, DMSO was added to dissolve it, and initiator AIBN (0.1 g) was added. Under nitrogen conditions, the reaction bottle was placed in a 70 ° C oil bath and stirred for reaction for 24 hours. After the reaction was completed, it was placed in a dialysis bag for dialyzation for 3 days and then freeze-dried to obtain polydimethylaminoethyl methacrylate PDM2.
[0039] Example 3: Purified dimethylaminoethyl methacrylate (50 g) was placed in a 250 mL reaction bottle, tetrahydrofuran was added to dissolve it, and initiator AIBN (0.02 g) was added. Under nitrogen conditions, the reaction bottle was placed in a 70 ° C oil bath and stirred for reaction for 24 h. After the reaction was completed, it was placed in a dialysis bag for dialyzation for 3 days and then freeze-dried to obtain polydimethylaminoethyl methacrylate PDM3.
[0040] Example 4: Purified dimethylaminoethyl methacrylate (50 g) was placed in a 250 mL reaction bottle, DMSO was added to dissolve, and initiator AIBN (0.06 g) was added. Under nitrogen conditions, the reaction bottle was placed in a 40 ° C oil bath and stirred for reaction for 24 hours. After the reaction was completed, it was placed in a dialysis bag for dialyzation for 3 days and then freeze-dried to obtain polydimethylaminoethyl methacrylate PDM4.
[0041] Example 5: Purified dimethylaminoethyl methacrylate (50 g) was placed in a 250 mL reaction bottle, DMSO was added to dissolve it, and initiator AIBN (0.06 g) was added. Under nitrogen conditions, the reaction bottle was placed in an 85 ° C oil bath and stirred for reaction for 24 hours. After the reaction was completed, it was placed in a dialysis bag for dialyzation for 3 days, and then freeze-dried to obtain polydimethylaminoethyl methacrylate PDM5.
[0042] Example 6: Purified dimethylaminoethyl methacrylate (50 g) was placed in a 250 mL reaction bottle, DMSO was added to dissolve it, and initiator AIBN (0.06 g) was added. Under nitrogen conditions, the reaction bottle was placed in a 70 ° C oil bath and stirred for reaction for 5 hours. After the reaction was completed, it was placed in a dialysis bag for dialyzation for 3 days, and then freeze-dried to obtain polydimethylaminoethyl methacrylate PDM6.
[0043] Example 7: Purified dimethylaminoethyl methacrylate (50 g) was placed in a 250 mL reaction bottle, DMSO was added to dissolve it, and initiator AIBN (0.06 g) was added. Under nitrogen conditions, the reaction bottle was placed in a 70 ° C oil bath and stirred for reaction for 96 hours. After the reaction was completed, it was placed in a dialysis bag for dialyzation for 3 days and then freeze-dried to obtain polydimethylaminoethyl methacrylate PDM7.
[0044] Example 8: Purified dimethylaminoethyl methacrylate (50 g) was placed in a 250 mL reaction bottle, tetrahydrofuran was added to dissolve it, and initiator AIBN (0.06 g) was added. Under nitrogen conditions, the reaction bottle was placed in a 70 ° C oil bath and stirred for reaction for 24 h. After the reaction was completed, it was placed in a dialysis bag for dialyzation for 3 days, and then freeze-dried to obtain polydimethylaminoethyl methacrylate PDM8.
[0045] The preparation of polydimethylaminoethyl methacrylate in the above-mentioned Examples 1 to 8, the specific data are shown in Table 1.
[0046] As shown in the table below, when the amount of catalyst AIBN is 0.1%, the reaction time is 24 h, the reaction temperature is 70 °C, and the reaction solvent is dimethyl sulfoxide, the obtained poly (dimethylaminoethyl methacrylate) M w The reaction conditions are as follows: the molecular weight is 41.3k, the PDI is 1.55, the molecular weight is relatively high, and the molecular weight distribution is relatively narrow.
[0047] Table 1 sample Reaction temperature / ℃ AIBN / % Reaction time / h Reaction solvent <![CDATA[ M w ]]> PDI <![CDATA[PDM1]]> 70 0.1 24 DMSO 41.9k 1.55 <![CDATA[PDM2]]> 70 0.2 24 DMSO 47.2k 2.41 <![CDATA[PDM3]]> 70 0.04 24 DMSO 32.4k 2.36 <![CDATA[PDM4]]> 40 0.1 24 DMSO 22.7k 1.83 <![CDATA[PDM5]]> 85 0.1 24 DMSO 46.8k 2.11 <![CDATA[PDM6]]> 70 0.1 5 DMSO 8.2k 2.43 <![CDATA[PDM7]]> 70 0.1 96 DMSO 43.2k 1.92 <![CDATA[PDM8]]> 70 0.1 24 THF 28.9k 2.53 .
[0048] Example 9: According to the weight percentage, the raw materials of polypropylene and poly(dimethylaminoethyl methacrylate) (PDM1) were weighed and placed in an oven at 100°C for 12 h, and then placed in a mixer to mix evenly; the mixed materials were then added to a twin-screw extruder, melt blended at 200°C and 160 r / min, and extruded into granules to obtain a polymer composition PP-PDM1. The specific data are shown in Table 2.
[0049] Table 2 sample PP / % <![CDATA[PDM1 / %]]> <![CDATA[PP-PDM1-1]]> 95 5 <![CDATA[PP-PDM1-2]]> 92 8 <![CDATA[PP-PDM1-3]]> 90 10 <![CDATA[PP-PDM1-4]]> 80 20 <![CDATA[PP-PDM1-5]]> 70 30 .
[0050] Example 10: According to the weight percentage, the raw materials of polypropylene and poly(dimethylaminoethyl methacrylate) (PDM2) were weighed and placed in an oven at 100°C for 12 h, and then placed in a mixer to mix evenly; the mixed materials were then added to a twin-screw extruder, melt blended at 200°C and 160 r / min, and extruded into granules to obtain a polymer composition PP-PDM2. The specific data are shown in Table 3.
[0051] Table 3 sample PP / % <![CDATA[PDM2 / %]]> <![CDATA[PP-PDM2-1]]> 95 5 <![CDATA[PP-PDM2-2]]> 92 8 <![CDATA[PP-PDM2-3]]> 90 10 <![CDATA[PP-PDM2-4]]> 80 20 <![CDATA[PP-PDM2-5]]> 70 30 .
[0052] Example 11: According to the weight percentage, the raw materials of polypropylene and poly(dimethylaminoethyl methacrylate) (PDM3) were weighed and placed in an oven at 100°C for 12 h, and then placed in a mixer to mix evenly; the mixed materials were then added to a twin-screw extruder, melt blended at 200°C and 160 r / min, and extruded into granules to obtain a polymer composition PP-PDM3. The specific data are shown in Table 4.
[0053] Table 4 sample PP / % <![CDATA[PDM2 / %]]> <![CDATA[PP-PDM3-1]]> 95 5 <![CDATA[PP-PDM3-2]]> 92 8 <![CDATA[PP-PDM3-3]]> 90 10 <![CDATA[PP-PDM3-4]]> 80 20 <![CDATA[PP-PDM3-5]]> 70 30 .
[0054] Example 12: According to the weight percentage, the raw materials of polypropylene and poly(dimethylaminoethyl methacrylate) (PDM4-PDM8) were weighed and placed in an oven at 100°C for 12 h, and then placed in a mixer to mix evenly; the mixed materials were then added to a twin-screw extruder, melt blended at 200°C and 160 r / min, and extruded into granules to obtain the corresponding polymer composition. The specific data are shown in Table 5.
[0055] Table 5 sample PP / % <![CDATA[PDM2 / %]]> sample PP / % <![CDATA[PDM2 / %]]> <![CDATA[PP-PDM4-1]]> 95 5 <![CDATA[PP-PDM6-2]]> 90 10 <![CDATA[PP-PDM4-2]]> 90 10 <![CDATA[PP-PDM7-1]]> 95 5 <![CDATA[PP-PDM5-1]]> 95 5 <![CDATA[PP-PDM7-2]]> 90 10 <![CDATA[PP-PDM5-2]]> 90 10 <![CDATA[PP-PDM8-1]]> 95 5 <![CDATA[PP-PDM6-1]]> 95 5 <![CDATA[PP-PDM8-2]]> 90 10 .
[0056] Example 13: The polymer compositions of Example 9, Example 10, Example 11 and Example 12 were melted by heating, and the melt passed through the die head, and after stretching and shaping, the shape of a culture dish was formed under the action of the mold, and cooled and shaped to obtain a culture dish with cell adhesion. Among them, the preheating temperature for stretching is 110°C, the stretching temperature is 125°C, the stretching ratio is 4.5 times, and the shaping temperature is 240°C.
[0057] Example 14: MCF7 cells (MCF7-GFP) that constantly express green fluorescent protein were cultured using Example 13 and a commercial cell culture dish, and continuous cell culture was performed in an incubator containing 10% fetal bovine serum and 5% carbon dioxide by volume. The proliferation of MCF7-GFP cells was observed under a fluorescence microscope.
[0058] Depend on Figure 3 It can be seen that when the initial number of cells is the same, after the same culture time, the number of cells expressing fluorescent protein in the PP-PDM1-3 group is the largest, indicating that PP-PDM1-3 is more suitable for cell growth and proliferation than commercial culture plates.
[0059] Note that the above are only preferred embodiments of the present invention and the technical principles used. Those skilled in the art will understand that the present invention is not limited to the specific embodiments described herein, and that various obvious changes, readjustments and substitutions can be made by those skilled in the art without departing from the scope of protection of the present invention. Therefore, although the present invention has been described in more detail through the above embodiments, the present invention is not limited to the above embodiments, and may include more other equivalent embodiments without departing from the concept of the present invention, and the scope of the present invention is determined by the scope of the appended claims.
Claims
1. A method for preparing a polymer functional material with cell adhesion, characterized in that: The following steps are involved: A. Preparation of polydimethylaminoethyl methacrylate: A1. Filter and purify dimethylaminoethyl methacrylate using a neutral alumina column to remove the polymerization inhibitor in its industrial product; A2, adding purified dimethylaminoethyl methacrylate monomer and initiator azobisisobutyronitrile into a reaction vessel, dissolving them in an organic solvent, and heating and stirring to react; A3, after the reaction is completed, place in a dialysis bag for 120 h, freeze-dry, and obtain poly (dimethylaminoethyl methacrylate); B. Preparation of polymer functional materials with cell adhesion by melt blending: B1, fully mixing polypropylene and the prepared polydimethylaminoethyl methacrylate according to a mass ratio, drying and grinding into powder to obtain a blend; B2, adding the blend into a twin-screw extruder, melt blending at 170-240° C., 160-300 r / min, and extruding granulation; B3. The product obtained in step B2 is sequentially stretched and heat-set to obtain a culture dish with cell adhesion.
2. The method for preparing a polymer functional material with cell adhesion according to claim 1, characterized in that: In step A2, the amount of the initiator azobisisobutyronitrile is 0.04%-0.2%, the reaction time is 5-96 h, and the reaction temperature is 40-85°C.
3. The method for preparing a cell-adhesive polymer functional material according to claim 2, characterized in that: The dosage of the azobisisobutyronitrile is 0.1%.
4. The method for preparing a polymer functional material with cell adhesion according to claim 2, characterized in that: The reaction time is 24 hours and the reaction temperature is 70°C.
5. The method for preparing a polymer functional material with cell adhesion according to claim 1, characterized in that: In step A2, the organic solvent is one or more of dimethyl sulfoxide, N,N-dimethylformamide, toluene and tetrahydrofuran.
6. The method for preparing a polymer functional material with cell adhesion according to claim 1, characterized in that: The organic solvent is dimethyl sulfoxide.
7. The method for preparing a polymer functional material with cell adhesion according to claim 1, characterized in that: In step A3, the dialysis freeze-drying process uses a dialysis bag with a molecular weight cut-off of 500-50000 Da.
8. The method for preparing a polymer functional material with cell adhesion according to claim 1, characterized in that: In step B3, the preheating temperature for stretching is 100-150°C, the stretching temperature is 120-160°C, the stretching multiple is 4-6 times; and the setting temperature is 230-245°C.
9. A polymer functional material with cell adhesion, characterized in that: The method according to claim 1 is used for preparing the polypropylene, which is composed of the following raw materials by mass percentage: polypropylene: 70-95%, polydimethylaminoethyl methacrylate: 5-30%; wherein the polypropylene is at least one of homopolypropylene and copolymer polypropylene.
10. An application of a polymer functional material with cell adhesion according to claim 1, characterized in that: The method can be used for cell culture. The prepared high molecular functional material with cell adhesion is melted by heating, and the melt passes through a die head to form a culture dish shape under the action of the mold, and is cooled and shaped to obtain a culture dish with cell adhesion.
Citation Information
Patent Citations
Method for improving hydrophilicity of polypropylene and application of obtained product
CN102336960A
Resin composition, substrate, and cell culture method
CN108779338A
Modified polyethylene film for cell therapy liquid storage bag and preparation method of modified polyethylene film
CN114456529A
Polymer material surface treatment method for promoting cell adherence
CN116005445A
Bag for cell culture
JP1991065177A