Gel microtube and preparation method thereof
Through the combination of water-soluble and water-insoluble polymers, spray spraying and solvent leaching technology are used to prepare hydrogel microtubes with high ductility and high stability, which solves the problem of difficult small tube diameter and poor stability in water, and achieves the problem of Application of hydrogel microtubes in water for long-term stability.
Patent Information
- Application Number
- CN202411186579.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The prior art is difficult to prepare hydrogel microtubes less than 4 mm, and the hydrogel has poor stability and low mechanical strength when immersed in water for a long time, which limits its application in the fields of drug release, tissue engineering and in vitro cell culture.
Using a combination of water-soluble and water-insoluble polymers, gel microtubes are prepared by spray spraying and solvent leaching techniques to form hydrogel materials with high ductility and Young's modulus, and to improve them by heat treatment and rehydration steps. Structural stability.
Long-term stable hydrogel microtube preparation in water is achieved, with a ductility rate greater than 100%, and Young's modulus is within the range of 100kPa-5 MPa. It can maintain stability in water and is suitable for biomedical applications.
Smart Images

Figure CN119081325A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to a gel microtube and a preparation method thereof. Background Art
[0002] Hydrogel microtubes have wide applications and research value in the fields of drug release, tissue engineering, bionic organs and in vitro cell culture, but there are some technical problems that limit their development and application. First, the preparation of hydrogel microtubes with controllable structures is a technical challenge, especially in the preparation of small-diameter microtubes (less than 4 mm in diameter). In the currently disclosed technology, the prepared gel microtubes are large in size, and microtubes with a diameter of less than 4 mm are difficult to prepare. Secondly, the storage stability of the gel microtubes in water. The stability of hydrogel materials is crucial to their service life, especially when immersed in water or tissue fluid for a long time. However, long-term immersion of existing gel microtubes in water will cause the microtubes to swell, and the structural strength of the tube wall will be significantly reduced. In addition, the mechanical strength of hydrogel microtubes is low, which is limited by the strength of the hydrogel, which limits the structural stability of the gel. These problems need to be studied and solved in order to better apply hydrogel microtubes.
[0003] At present, CN115814152A discloses a method for preparing a high-strength interpenetrating network hydrogel blood vessel with a directional fiber microstructure, that is, firstly using 3D printing technology to quickly prepare an IPN hydrogel tube, and then using a homemade fixture to restrictively air-dry the tubular hydrogel. During the dehydration process, stress will be generated in a specific direction inside the hydrogel, and the polymer will gradually form a hierarchical directional fiber structure under the action of stress. This structure can still be maintained after the hydrogel is rehydrated, greatly improving the strength of the blood vessel. In addition, CN106810704A discloses a method for preparing a polyvinyl alcohol hydrogel. When preparing a polyvinyl alcohol solution, a properly proportioned DMSO and DMF mixture is used as a solvent, so that the resulting polyethylene solution does not need to undergo a repeated cycle of freezing-thawing, and the polyvinyl alcohol hydrogel can be obtained by simply standing and cooling naturally, and the resulting polyvinyl alcohol hydrogel has excellent mechanical strength. Then, a microtube with controllable structure can be obtained by mold manufacturing.
[0004] Although hydrogel microtube technology has been reported, the related technology requires complex photocuring molding or involves the use of biotoxic organic solvents, and current technical research does not involve the long-term stability of hydrogel microtubes, especially the stability in water immersion environments. Summary of the invention
[0005] Aiming at the problem that the preparation technology of tubular structure gel is complicated and small diameter gel microtubes are difficult to prepare, the present invention provides a gel microtube.
[0006] Specifically, a gel microtube has a tube wall thickness of 0.02mm-2mm and a tube diameter of 0.02-100mm; the water content of the hydrogel in the tube wall is 20%-95%, and the hydrogel is prepared from 10-60 parts of a water-soluble polymer, 10-60 parts of a water-insoluble polymer, 0-10 parts of a filler, 0-5 parts of an auxiliary agent and 20-80 parts of water as main components.
[0007] The wall thickness of the gel microtube is preferably 0.02 mm-1 mm, and the tube diameter is 0.02-4 mm.
[0008] The elongation of the hydrogel microtube is greater than 100%, and the Young's modulus is 100 kPa-5 MPa.
[0009] In the present invention, the water-soluble polymer is a polymer that can absorb water to form a gel structure, and contains hydroxyl, amide or carboxyl functional groups, and can be one or more combinations of polyvinyl alcohol, polyacrylic acid, sodium polyacrylate, polyhydroxyethyl acrylate, water-soluble cellulose, sodium alginate and chitosan.
[0010] Among them, the non-water-soluble polymer can interact with the water-soluble polymer to form hydrogen bond interactions, electrostatic interactions, hydrophobic interactions, etc., thereby forming a stable hydrophilic-hydrophobic interface and increasing the structural stability of the water-soluble polymer. It can be one or more combinations of polyethylene-vinyl acetate copolymer, polyurethane, polytetrafluoroethylene, silicone and fluoroelastomer, etc.
[0011] Furthermore, the water-insoluble polymer is an aqueous emulsion to increase the uniformity of the water-insoluble polymer and the water-soluble polymer during the mixing process and promote the formation of a stable phase separation.
[0012] The filler increases the structural strength of the gel, promotes the gel to form a stable polymer network, and plays a role in enhancing the mechanical properties of the gel. It can be an inorganic material for adjusting the structural strength and stability of the gel, and can be one or more of silicon dioxide, magnesium oxide, aluminum oxide, diatomaceous earth and magnesium aluminum hydrotalcite.
[0013] Among them, the auxiliary agent increases the stability of the preparation process system, avoids the instability and phase separation of the mixed liquid system, and extends the process operation time; secondly, the auxiliary agent also increases the surface smoothness of the gel molding, reduces the interface adhesion and other effects, and can be a surfactant, such as polyvinyl pyrrolidone, F127, etc., or small molecule alcohols, such as ethanol, isopropanol, ethylene glycol or propylene glycol. One or more.
[0014] Another object of the present invention is to provide a method for preparing the above-mentioned gel microtube.
[0015] Specifically, the preparation method of the gel microtube comprises the following steps:
[0016] S1: 10-60 parts of a water-soluble polymer, 10-60 parts of a water-insoluble polymer, 0-10 parts of a filler, 0-5 parts of an additive and 20-80 parts of water are taken to prepare a gel precursor solution;
[0017] S2: coating the template surface with gel precursor solution;
[0018] S3: solvent leaching: immersing the template coated with the gel precursor solution in the solvent;
[0019] S4: heat treatment; increase the gel polymer to form a microphase interface;
[0020] S5: rehydration; soaking the heat-treated gel microtube semi-finished product in water for rehydration to form a gel;
[0021] S6: Remove the template to obtain the gel microtube.
[0022] The template of the present invention needs to be surface treated before coating. That is, a water-soluble polymer is coated on the surface of the template to form a transfer layer, which increases the adhesion of the gel precursor on the template surface and helps to rehydrate and remove the template. The water-soluble polymer can be one or more of polyethylene glycol, polyvinyl pyrrolidone, polyvinyl alcohol, polyacrylamide, etc. The polymer used to modify the template surface is required to have good water solubility and good film-forming properties, and can form a uniform and delicate polymer thin layer on the template surface. In addition, during the heat treatment of step S4, the water-soluble polymer modified on the template surface can be dissolved in water, so that the hydrated gel microtubes can be removed from the template surface by physical peeling.
[0023] The template surface treatment can be achieved by solution dipping. The concentration of the water-soluble polymer solution used for dipping is 1%-5%, and then it is dried to form a modification layer on the template surface. The drying temperature is 60-120 degrees.
[0024] The template material can be glass, metal, ceramic or organic resin, etc. The template shape can be cylindrical, surface threaded or other structures, that is, the shape of the template determines the internal shape of the gel microtube. The diameter of the template is 10 microns-50 mm.
[0025] In step S1, the solid content of the gel precursor solution is 10%-50%.
[0026] In step S2, the coating is performed by spray coating, electrospray coating or dip coating. The present invention preferably uses spray coating. In spray coating, the liquid flow rate is 1-20 mL / min; the gas flow rate is 1-20 L / min; the temperature of the precursor solution, the environment and the template surface is 35-85 degrees; and the spraying time is 1-50 minutes. Furthermore, in order to improve the uniformity of the spraying, the template is placed on an automatic rotating traction table with a rotation speed of 10 rpm-120 rpm.
[0027] In step S3, the gel precursor still has fluidity after being sprayed onto the template surface, and under the action of gravity, the wall thickness of the gel microtubes will be uneven. Therefore, the present invention uses solvent leaching treatment to quickly fasten the sprayed gel precursor to the template surface. The solvent used is a mixed solution of alcohols, etc., including one or more of alcohols such as ethanol, isopropanol or ethylene glycol, and esters such as ethyl acetate, ethyl acetoacetate, n-butyl acetate, etc., and the ratio of alcohol to ester is 5:1-1:5. The solvent leaching time is 1-10 minutes.
[0028] In step S4, oven drying is adopted, and the oven temperature is 60-120 degrees and the heating time is 30 minutes to 24 hours.
[0029] In step S5, the soaking temperature is 20-50 degrees, and the soaking time is 30 minutes to 24 hours.
[0030] The beneficial effects of the present invention compared with the prior art are as follows:
[0031] 1. The tube wall of the gel microtube provided by the present invention is a hydrogel material, that is, a polymer composite material containing water, the tube wall thickness is 0.02mm-2mm, and the tube diameter is 0.02-100mm; the water content of the hydrogel in the tube wall is 20%-95%; the ductility of the gel microtube is greater than 100%; the Young's modulus of the gel microtube is 100kPa-5 MPa.
[0032] 2. The gel microtubes provided by the present invention are stable when immersed in water, physiological saline or culture medium. After one week of immersion, the mass change rate of the microtubes is less than 10%, and the change rates of the microtube diameter and wall size are less than 10%.
[0033] 3. The hydrogel provided in the present invention can be used to prepare both large-diameter gel microtubes and small-diameter gel microtubes with a diameter of less than 4 mm and a wall thickness of less than 1 mm.
[0034] 4. The gel microtube provided by the present invention can be used as an artificial biological tissue substitute, can be used for biological pipelines such as artificial blood vessels and artificial trachea, and can be used for biomedicine or biological teaching tools.
[0035] 5. The hydrogel provided in the present invention can be suitable for long-term stable use in water.
[0036] Controlling the hydrogel polymer network to form a hydrophilic and hydrophobic two-phase structure is the basic principle of hydrogel anti-swelling, and realizes the preparation of hydrogels that can be stable in water for a long time. Therefore, the focus of the present invention is how to promote the formation of a strong interactive two-phase interface and a structurally stable two-phase structure between water-soluble polymers and water-insoluble polymers.
[0037] (1) Type of hydrophilic polymer. The hydrophilic polymer absorbs water to form a fluffy network, which is the prerequisite for the formation of hydrogel. Without the hydrophilic polymer, gel cannot be formed. However, the unlimited swelling of the hydrophilic polymer until it dissolves is also the fundamental reason that restricts the long-term use of hydrogel in water. The hydrophilic polymer selected in the present invention is a polymer containing hydroxyl, amide or carboxyl functional groups, which can be partially hydrated in water to form a gel. At the same time, the interaction between polymer chains and the presence of hydrophobic microphases of polymer chains limit their complete dissolution in water.
[0038] (2) Formation of hydrophilic-hydrophobic interface. The introduction of non-water-soluble polymers can form a hydrophilic-hydrophobic interface with the water-soluble polymer. The result of this action is similar to anchoring the water-soluble polymer molecular chain to the periphery of the non-water-soluble polymer through the hydrophilic-hydrophobic interface to form a continuous hydrophilic-hydrophobic network. The formation of this hydrophilic-hydrophobic interface is during step S4, by drying to remove water, and the mixed solution forms a solid film. During the hydration process of step S5, the water-soluble polymer can absorb water again to form a gel, while the non-water-soluble polymer cannot be rehydrated, thus forming a hydrogel network supported by the non-water polymer.
[0039] (3) Introduction of fillers: The fillers of the present invention can be filled in the polymer network to improve the structural stability of the gel and increase the mechanical strength of the gel.
[0040] (4) Selection of additives. Additives are used to promote the formation of hydrophilic-hydrophobic interfaces. Additives increase the stability of water-soluble polymer and water-insoluble polymer emulsions, improve the dispersion stability of fillers in them, avoid phase separation between the two, and help form a uniform and continuous two-phase microstructure.
[0041] (5) The hydrogel obtained by the present invention has excellent anti-swelling properties and can be stored or used in water for a long time. The elongation of the hydrogel is greater than 100%, the tensile stress at break is greater than 500 kP, and the Young's modulus is 50 kPa-5 MPa. The hydrogel can be immersed in water, physiological saline or biological culture fluid for a long time, and the immersion time exceeds 3 months. The mechanical properties of the gel before and after immersion remain stable, and the mass change rate before and after immersion is less than 10%.
[0042] 6. In the preparation method provided by the present invention, the adhesion of the gel of the outer coating material is increased by introducing a water-soluble modification layer, and at the same time, it is redissolved during hydration to increase the demolding efficiency and reduce the damage of the demolded gel microtubes, thereby realizing the preparation of gel microtubes with threaded inner walls.
[0043] 7. In the preparation method provided by the present invention, the strength of the gel microtubes is increased through two steps of solvent leaching and heat treatment, that is, the processing efficiency is improved, the tube wall forming time is reduced, and the tube wall strength is increased.
[0044] 8. The preparation method of the present invention is simple, the raw material cost is low, the mechanical strength is high, and it can be stably used for a long time in an aqueous medium or a biological liquid medium (tissue fluid, culture fluid, etc.). BRIEF DESCRIPTION OF THE DRAWINGS
[0045] Figure 1 The stress-strain relationship curves of polyvinyl alcohol hydrogels with different EVA contents.
[0046] Figure 2 The stress-strain relationship curves of cellulose hydrogels with different EVA contents.
[0047] Figure 3 The mass change of polyvinyl alcohol hydrogel when immersed in water.
[0048] Figure 4 The stress-strain changes of polyvinyl alcohol hydrogel when immersed in water.
[0049] Figure 5 Hydrogel microtubes with different diameters.
[0050] Figure 6 It is a hydrogel microtube with a spiral inner wall.
[0051] Figure 7 Hydrogel microtubes with different wall thicknesses. DETAILED DESCRIPTION
[0052] Example 1 Polyvinyl alcohol type hydrogel
[0053] 20 grams of polyvinyl alcohol was dissolved in water to obtain an aqueous solution with a mass concentration of 10%, and then 5 grams of magnesium oxide and 1 gram of polyvinyl pyrrolidone were added and mixed evenly to obtain a mixed solution 1.
[0054] Take 10 grams, 20 grams, 30 grams, 40 grams and 50 grams of polyethylene-vinyl acetate copolymer (EVA) and use an emulsion with a concentration of 50%.
[0055] Take 5 parts of mixed solution 1, mix them with the above 5 parts of EVA emulsion respectively, and then mechanically stir for 30 minutes at a stirring speed of 1000rpm to obtain 5 parts of mixed solution 2. Vacuum degas the 5 parts of mixed solution 2 for 10 minutes respectively. Use a scraper coater to coat the 5 parts of mixed solution 2 on the substrate to form a film. The scraper spacing is 100 microns, the coating speed is 600mm / min, and the coating substrate is glass. After coating, put it into a hot air oven to dry. The drying temperature is 70 degrees and the drying time is 120 minutes. Remove the dried film and soak it in pure water. The soaking temperature is 30 degrees and the soaking time is 2 hours to obtain a polyvinyl alcohol type hydrogel. The stress-strain curve of the obtained gel is shown in the attached figure. Figure 1 shown.
[0056] Example 2 Cellulose hydrogel
[0057] 20 grams of water-soluble cellulose was dissolved in water to obtain an aqueous solution with a mass concentration of 10%, and then 5 grams of magnesium oxide and 1 gram of polyvinyl pyrrolidone were added and mixed evenly to obtain a mixed solution 1.
[0058] Take 10 grams, 30 grams and 50 grams of polyethylene-vinyl acetate copolymer (EVA) and use an emulsion with a concentration of 50%.
[0059] Take 3 parts of mixed solution 1 and mix them with the above 3 parts of EVA emulsion respectively. Then stir mechanically for 30 minutes at a stirring speed of 1000rpm to obtain 3 parts of mixed solution 2. Degas the 3 parts of mixed solution 2 in vacuum for 10 minutes respectively. Use a scraper coater to coat the 3 parts of mixed solution 2 on the substrate to form a film. The scraper spacing is 100 microns, the coating speed is 600mm / min, and the coating substrate is glass. After coating, put it into a hot air oven to dry. The drying temperature is 70 degrees and the drying time is 120 minutes; remove the dried film and soak it in pure water at a soaking temperature of 30 degrees and a soaking time of 2 hours to obtain a cellulose hydrogel. The stress-strain curve of the gel is shown in the attached figure. Figure 2 shown.
[0060] Example 3 Long-term stability of polyvinyl alcohol hydrogel in water
[0061] The polyvinyl alcohol hydrogel containing 20 g of EVA in Example 1 was immersed in pure water at a temperature of 25 degrees. The mass of the gel after different immersion times was weighed, and the stress and strain of the gel before and after immersion were tested. The changes in gel mass are shown in the attached figure. Figure 3 The stress-strain of the gel is shown in the attached Figure 4 shown.
[0062] Example 4 Preparation of gel microtubes with different diameters and smooth inner walls
[0063] First, a gel precursor solution was prepared: 20 grams of polyvinyl alcohol was dissolved in water to obtain an aqueous solution with a mass concentration of 10%, and then 5 grams of magnesium oxide and 1 gram of polyvinyl pyrrolidone were added and mixed evenly; the obtained mixed solution was then mixed with 20 grams of polyethylene-vinyl acetate copolymer (EVA), and the EVA was added in the form of an emulsion with a concentration of 50%; then mechanical stirring was performed for 30 minutes at a stirring speed of 1000 rpm; and the mixed solution was vacuum degassed for 10 minutes.
[0064] Different cylindrical glass rods were used as templates, with diameters of 12 mm, 10 mm, 8 mm, 5 mm, 3 mm, 2 mm and 1 mm respectively; the length of the glass rod was 10 cm. Polyvinyl alcohol was used as a surface modifier, and the glass rod was immersed in a 2% polyvinyl alcohol solution, the excess liquid was drained, and then placed in an oven to dry at 60 degrees.
[0065] The gel precursor solution was sprayed onto the modified glass rod surface, with a liquid flow rate of 50 mL / min, a gas flow rate of 7 L / min, a gel precursor solution, an environment, and a template surface temperature of 55 degrees, and a spraying time of 15 minutes. The glass rod was placed on an automatic rotating traction table with a rotation speed of 60 rpm.
[0066] The sprayed glass rod was immersed in a mixed solution of ethanol and ethyl acetate in a volume ratio of 2:1 for 5 minutes, and then taken out and dried.
[0067] The glass rod was placed in an oven for heat treatment at 85 degrees for 12 hours. Then, it was taken out and soaked in pure water for 12 hours for rehydration at a water temperature of 25 degrees. The microtube was removed from the surface of the glass rod to obtain the gel microtube. Figure 5 Photos of hydrogel microtubes with different diameters.
[0068] Example 5 Preparation of Gel Microtubes with Threaded Inner Walls
[0069] First, a gel precursor solution was prepared: 20 grams of polyvinyl alcohol was dissolved in water to obtain an aqueous solution with a mass concentration of 10%, and then 5 grams of magnesium oxide and 1 gram of polyvinyl pyrrolidone were added and mixed evenly; the obtained mixed solution was then mixed with 20 grams of polyethylene-vinyl acetate copolymer (EVA), and the EVA was added in the form of an emulsion with a concentration of 50%; then mechanical stirring was performed for 30 minutes at a stirring speed of 1000 rpm; and the mixed solution was vacuum degassed for 10 minutes.
[0070] A stainless steel rod with a surface thread was selected as the template, with a rod diameter of 3 mm and a rod length of 10 cm. Polyvinyl alcohol was used as a surface modifier, and the template rod was immersed in a 2% polyvinyl alcohol solution, the excess liquid was drained, and then placed in an oven for drying at 60 degrees.
[0071] The gel precursor solution was sprayed onto the modified glass rod surface at a liquid flow rate of 50 mL / min and a gas flow rate of 7 L / min. The temperature of the gel precursor solution, the environment and the template surface was 55 degrees. The spraying time was 15 minutes. The template rod was placed on an automatic rotating traction table with a rotation speed of 60 rpm.
[0072] The sprayed template rod was immersed in a mixed solution of ethanol and ethyl acetate in a volume ratio of 2:1 for 5 minutes, and then taken out and dried.
[0073] The rod was placed in an oven for heat treatment at 85 degrees for 12 hours. Then it was taken out and soaked in pure water for 12 hours for rehydration at a water temperature of 25 degrees. The microtube was removed from the template surface to obtain the gel microtube. Figure 6 This is a photo of a hydrogel microtube with a thread-like inner wall.
[0074] Example 6 Preparation of gel microtubes with different wall thicknesses
[0075] First, a gel precursor solution was prepared: 20 grams of polyvinyl alcohol was dissolved in water to obtain an aqueous solution with a mass concentration of 10%, and then 5 grams of magnesium oxide and 1 gram of polyvinyl pyrrolidone were added and mixed evenly; the obtained mixed solution was then mixed with 20 grams of polyethylene-vinyl acetate copolymer (EVA), and the EVA was added in the form of an emulsion with a concentration of 50%; then mechanical stirring was performed for 30 minutes at a stirring speed of 1000 rpm; and the mixed solution was vacuum degassed for 10 minutes.
[0076] Different cylindrical glass rods were used as templates, with diameters of 2 mm and lengths of 10 cm. Polyvinyl alcohol was used as a surface modifier, and the glass rods were immersed in a 2% polyvinyl alcohol solution, the excess liquid was drained, and then placed in an oven to dry at 60 degrees.
[0077] The gel precursor solution was sprayed onto the modified glass rod surface, with a liquid flow rate of 50 mL / min, a gas flow rate of 7 L / min, a gel precursor solution, an environment, and a template surface temperature of 55 degrees, and a spraying time of 15 minutes and 30 minutes, respectively. The glass rod was placed on an automatic rotating traction table with a rotation speed of 60 rpm.
[0078] The sprayed glass rod was immersed in a mixed solution of ethanol and ethyl acetate in a volume ratio of 2:1 for 5 minutes, and then taken out and dried.
[0079] The glass rod was placed in an oven for heat treatment at 85 degrees for 12 hours. Then, it was taken out and soaked in pure water for 12 hours for rehydration at a water temperature of 25 degrees. The microtube was removed from the surface of the glass rod to obtain the gel microtube. Figure 7 Photos of hydrogel microtubes with different wall thicknesses obtained with spraying times of 15 min and 30 min, respectively.
Claims
1. A gel microtube, characterized in that: The tube wall thickness is 0.02mm-2mm, and the tube diameter is 0.02-100mm; the water content of the hydrogel of the tube wall is 20%-95%, and the hydrogel is prepared from the hydrogel with 10-60 parts of water-soluble polymer, 10-60 parts of water-insoluble polymer, 0-10 parts of filler, 0-5 parts of auxiliary agent and 20-80 parts of water as main components.
2. The gel microtube according to claim 1, characterized in that: The water-soluble polymer is a polymer containing a hydroxyl group, an amide group or a carboxyl group; the water-insoluble polymer is one or more combinations of polyethylene-vinyl acetate copolymer, polyurethane, polytetrafluoroethylene, silicone and fluoroelastomer.
3. The gel microtube according to claim 2, characterized in that: The water-soluble polymer is one or more combinations of polyvinyl alcohol, polyacrylic acid, sodium polyacrylate, polyhydroxyethyl acrylate, water-soluble cellulose, sodium alginate and chitosan.
4. The gel microtube according to claim 2, characterized in that: The water-insoluble polymer is an aqueous emulsion.
5. The gel microtube according to claim 1, characterized in that: The filler is one or more combinations of silicon dioxide, magnesium oxide, aluminum oxide, diatomaceous earth and magnesium aluminum hydrotalcite; the auxiliary agent is a surfactant or a small molecule alcohol.
6. The method for preparing the gel microtube according to any one of claims 1 to 5, characterized in that: The following steps are involved: S1: 10-60 parts of a water-soluble polymer, 10-60 parts of a water-insoluble polymer, 0-10 parts of a filler, 0-5 parts of an additive and 20-80 parts of water are taken to prepare a gel precursor solution; S2: coating the template surface with gel precursor solution; S3: solvent leaching: immersing the template coated with the gel precursor solution in the solvent; S4: heat treatment; increase the gel polymer to form a microphase interface; S5: rehydration; soaking the heat-treated gel microtube semi-finished product in water for rehydration to form a gel; S6: Remove the template to obtain the gel microtube.
7. The method for preparing gel microtubes according to claim 6, characterized in that: The template needs to be surface treated before coating, and a water-soluble polymer is coated on the surface of the template to form a transfer layer.
8. The method for preparing gel microtubes according to claim 7, characterized in that: The water-soluble polymer is one or more of polyethylene glycol, polyvinyl pyrrolidone, polyvinyl alcohol and polyacrylamide; the template surface treatment is achieved by solution dipping, the concentration of the water-soluble polymer solution used for dipping is 1%-5%, and the drying temperature is 60-120 degrees.
9. The method for preparing gel microtubes according to claim 6, characterized in that: In the step S1, the solid content of the gel precursor solution is 10%-50%; in the step S2, the coating is performed by spray coating, electrospray coating or dipping; in the step S3, the solvent used comprises alcohols and esters, and the ratio of the alcohols to the esters is 5:1-1:5; the solvent leaching time is 1-10 minutes; in the step S4, oven drying is performed, and the oven temperature is 60-120 degrees; the heating time is 30 minutes-24 hours; in the step S5, the immersion temperature is 20-50 degrees, and the immersion time is 30 minutes-24 hours.
10. The method for preparing gel microtubes according to claim 9, characterized in that: The step S2 adopts spray coating, the liquid flow rate is 1-20mL / min, the gas flow rate is 1-20L / min, the gel precursor solution, the environment and the template surface temperature are 35-85 degrees; the spraying time is 1-50 minutes; the template is placed on an automatic rotating traction table, and the rotation speed is 10rpm-120rpm; in the step S3, the alcohol is one or more of ethanol, isopropanol and ethylene glycol; the ester is one or more of ethyl acetate, ethyl acetoacetate and n-butyl acetate.
Citation Information
Patent Citations
Polyvinyl alcohol hydrogel, method for preparing same and application of polyvinyl alcohol hydrogel
CN106810704A