Enhanced sound insulation film resin and preparation method thereof

By combining UV-resistant reinforced rubber and flame-retardant agel in the sound insulation film resin to form a cross-linked network structure, the shortcomings of existing sound insulation film resins in sound insulation, mechanics, UV-resistant and flame-retardant are solved, and better results are achieved The sound insulation and flame retardant properties meet the needs of use in various environments.

CN119081329APending Publication Date: 2024-12-06YINIAN OPTICAL MATERIALS MANUFACTURING (BAODING) CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411364410.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing sound insulation film resins have shortcomings in sound insulation effect, mechanical properties, UV resistance and flame retardant capabilities, and are difficult to meet the needs of use in various environments.

Method used

Using the combination of UV-resistant reinforced rubber and flame retardant agel, the interaction between nano zinc oxide and perylene modified nitrile rubber and phosphorylation can be obtained to form a cross-linked network structure, which enhances the toughness of sound insulation film resin and Flame retardant properties, and a sound insulation film resin with excellent sound insulation effect was prepared through extrusion granulation process.

Benefits of technology

It significantly improves the sound insulation effect, mechanical properties, UV resistance and flame retardant capabilities of sound insulation film resin, extends service life, and provides higher safety and sound insulation performance in flammable environments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081329A_ABST
    Figure CN119081329A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of sound insulation resin materials, and discloses enhanced sound insulation film resin and a preparation method thereof, the enhanced sound insulation film resin comprises the following raw materials: polyvinyl butyral, uvioresistant reinforced rubber, flame-retardant aerogel, a plasticizer and an antioxidant; the anti-ultraviolet reinforcing rubber and the flame-retardant aerogel are prepared to participate in the preparation process of the sound-insulating film resin, so that the prepared sound-insulating film resin has excellent sound-insulating effect, mechanical property, anti-ultraviolet capability and flame-retardant capability, and can effectively prevent and treat noise; the sound-insulation film resin prepared by the preparation method disclosed by the invention can be used for preparing the sound-insulation film resin, can prevent fire from spreading when a fire disaster occurs, can meet the use requirements in an inflammable environment, is not easy to age, crack and damage in the production and use processes, and has very long service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of sound insulation resin materials, and in particular to a reinforced sound insulation film resin and a preparation method thereof. Background Art

[0002] With the fast-paced development of modern society and the continuous acceleration of urbanization, noise pollution has become one of the main problems affecting people's quality of life. Being in a noisy environment for a long time not only disturbs people's daily life and erodes their physical and mental health, but may also lead to reduced work efficiency and create safety hazards. Therefore, the prevention and control of noise is an issue that needs to be urgently addressed at this stage.

[0003] Sound insulation materials are the main means of preventing and controlling noise. Common sound insulation materials on the market currently include glass, rubber, foam plastics and resins. Among them, resin materials have been widely used in the field of sound insulation materials due to their good processing performance and designability. However, ordinary sound insulation film resin materials still have many shortcomings in sound insulation effect, and the sound insulation effect needs to be improved. In addition, the mechanical properties and UV resistance are poor. During the production and use process, the strength and toughness are insufficient and it is easy to be damaged. The aging process is accelerated under ultraviolet radiation, which seriously affects the service life. At the same time, ordinary sound insulation film resins do not have flame retardant properties. When a fire occurs, there is a risk of fire spreading, and the possibility of its use in flammable environments is limited.

[0004] The patent with announcement number CN109762491B discloses a sound-insulating polyvinyl butyral film and a preparation method thereof. By adding four-needle zinc oxide whiskers, the sound insulation effect of the laminated glass made of the prepared sound-insulating polyvinyl butyral film is more than doubled, and has good sound insulation effect. However, the flame retardant performance of the sound-insulating polyvinyl butyral film prepared by the patent is average, thus limiting its use in flammable environments. Summary of the invention

[0005] The purpose of the present invention is to provide an enhanced sound insulation film resin and a preparation method thereof, which solves the following technical problems: (1) the sound insulation effect of ordinary sound insulation film resin needs to be improved, and it does not have flame retardant ability, which makes it difficult to meet the use requirements in various environments; (2) ordinary sound insulation film resin has general mechanical properties and poor UV resistance, which affects the service life.

[0006] The purpose of the present invention can be achieved by the following technical solutions:

[0007] A reinforced sound insulation film resin comprises the following raw materials in parts by weight:

[0008]

[0009] The anti-ultraviolet reinforcing rubber is prepared from nano zinc oxide and perylene-modified nitrile rubber; the perylene-modified nitrile rubber is prepared from amino-terminated liquid nitrile rubber and 3,4,9,10-perylenetetracarboxylic dianhydride;

[0010] The flame-retardant gas gel is prepared by fully mixing phosphorylated curdlan in distilled water and solidifying it through freeze drying; the phosphorylated curdlan is prepared by modified curdlan and triallyl phosphate under the action of an initiator; the modified curdlan is prepared by curdlan and acryloyl chloride.

[0011] Furthermore, the plasticizer is any one of triethylene glycol diisooctanoate, triethyl citrate, dibutyl sebacate, and dioctyl phthalate; and the antioxidant is any one of antioxidant 1010, antioxidant 3052, antioxidant 626, and antioxidant 1135.

[0012] Furthermore, the preparation method of the anti-ultraviolet reinforced rubber comprises the following steps:

[0013] S1: placing the amino-terminated liquid nitrile rubber and 3,4,9,10-perylenetetracarboxylic dianhydride in a three-necked flask in a constant temperature oil bath at 65-70° C., adding N,N-dimethylformamide, stirring thoroughly for 6-8 hours, cooling to room temperature, and collecting the product to obtain perylene-modified nitrile rubber;

[0014] S2: Place nano zinc oxide in toluene, disperse it by ultrasonic for 10-15 minutes, add perylene-modified nitrile rubber, heat it up with stirring, collect the product after cooling to room temperature, and obtain anti-ultraviolet reinforced rubber.

[0015] In this scheme, the amino group in the structure of the terminal amino liquid nitrile rubber reacts with the anhydride group in the structure of 3,4,9,10-perylenetetracarboxylic dianhydride to obtain perylene-modified nitrile rubber, and then the carboxyl group in the structure of the perylene-modified nitrile rubber interacts with the hydroxyl group on the surface of nano-zinc oxide to obtain an anti-UV reinforcing rubber. The anti-UV reinforcing rubber organicizes the surface of nano-zinc oxide, which can effectively prevent the agglomeration of nano-zinc oxide in the sound insulation film resin matrix, fully enhance the compatibility and dispersibility with the matrix material, and use liquid rubber as the main body to form a cross-linked network structure, which can significantly enhance the toughness of the sound insulation film resin. At the same time, the anti-UV reinforcing rubber structure also contains a perylene structure, which has rigidity and the ability to absorb ultraviolet rays, and can produce a synergistic effect with nano-zinc oxide, further improving the mechanical strength and anti-UV performance of the sound insulation film resin, so that it can meet the use requirements in various environments and have a long service life.

[0016] Furthermore, in step S1, the molecular weight of the amino-terminated liquid nitrile rubber is 9000-15000.

[0017] Furthermore, in step S2, the temperature of the heating and stirring is 100-108° C., and the time is 5-8 hours.

[0018] Furthermore, the method for preparing the flame-retardant gas gel comprises the following steps:

[0019] SS1: Place curdlan in deionized water, stir and mix thoroughly, add acryloyl chloride and catalyst, heat to 50-55°C and stir for 6-8h, remove low-boiling substances by vacuum distillation, and obtain modified curdlan;

[0020] SS2: Place the modified curdlan in N-methylpyrrolidone, add triallyl phosphate and initiator, heat to 55-60°C and stir for 8-10 hours, remove low-boiling substances by distillation under reduced pressure, and obtain phosphorylated curdlan;

[0021] SS3: Place the phosphated curdlan in distilled water, heat it to 45-50°C, stir it at a speed of 300-400r / min for 4-6h, solidify it after freeze-drying, and obtain a flame-retardant gel.

[0022] In this scheme, under the action of a catalyst, the hydroxyl groups in the curdlan structure react with the acyl chloride groups in the acryloyl chloride structure to obtain modified curdlan, and then under the action of an initiator, the alkenyl groups in the modified curdlan structure react with the multiple alkenyl groups in the triallyl phosphate structure to obtain a phosphated curdlan having a network structure, and then through the process of freeze-drying and curing treatment, a flame-retardant gas gel is obtained. The flame-retardant gas gel structure contains phosphate groups with excellent flame retardant effects, which can effectively prevent the spread and combustion of flames, so that the prepared sound insulation film resin material can meet the use requirements in a variety of flammable environments and improve the safety of use. At the same time, the flame-retardant gas gel has a unique cavity structure that can form more sound scattering and reflection interfaces, thereby effectively improving the sound insulation ability of the sound insulation film resin and making it have a more excellent sound insulation effect.

[0023] Furthermore, in step SS1, the catalyst is triethylamine.

[0024] Furthermore, in step SS2, the initiator is any one of azobisisobutyronitrile and azobisisoheptanenitrile.

[0025] A method for preparing an enhanced sound insulation film resin comprises the following steps:

[0026] Step 1: Place polyvinyl butyral, UV-resistant reinforcing rubber, flame-retardant gel, plasticizer, and antioxidant in a mixer and mix them evenly to obtain a mixture;

[0027] Step 2: Place the mixed material in a twin-screw extruder, set the screw speed to 300-500 r / min, the extrusion temperature to 200-220° C., melt-extrude and granulate to obtain a sound insulation film resin.

[0028] Beneficial effects of the present invention:

[0029] The present invention prepares anti-ultraviolet reinforcing rubber and flame-retardant gas gel in the preparation process of the sound insulation film resin, so that the prepared sound insulation film resin has excellent sound insulation effect, mechanical properties, anti-ultraviolet ability and flame retardant ability, can meet the use requirements in various environments, and is not easy to age and break during production and use, and has a very long service life.

[0030] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0031] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0032] Figure 1 This is a scanning electron microscope image of the flame-retardant gas gel of the present invention. DETAILED DESCRIPTION

[0033] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0034] The preparation methods of the anti-ultraviolet reinforced rubber and flame-retardant gas gel in the following examples and comparative examples of the present invention are as follows:

[0035] 1. Preparation of UV-resistant reinforced rubber

[0036] S1: 3 g of amino-terminated liquid nitrile rubber with a molecular weight of 9000 and 2.6 g of 3,4,9,10-perylenetetracarboxylic dianhydride were placed in a three-necked flask in a constant temperature oil bath at 65° C., 15 ml of N,N-dimethylformamide was added, and the mixture was stirred for 6 h. After cooling to room temperature, the product was collected to obtain perylene-modified nitrile rubber;

[0037] The acid-base titration method was used to test the carboxyl content in the perylene-modified nitrile rubber. 1 g of perylene-modified nitrile rubber was weighed as a sample and placed in 30 ml of acetone solution. An excess of 0.2 mol / L KOH-ethanol standard solution and 2 drops of phenolphthalein indicator were added. After sufficient stirring and mixing, 0.2 mol / L hydrochloric acid standard solution was used for back titration. After the color in the solution disappeared, stirring was continued for 30 min. After the color appeared, titration was continued. The operation was repeated until the color completely disappeared. At the same time, a blank experiment was performed to record the amount of alkali consumed and the amount of acid neutralized. The carboxyl content in the sample was calculated with reference to the following formula: Carboxyl content = c(V-V0)×45×100% / m; wherein c is the concentration of the hydrochloric acid standard solution, mol / L; V is the volume of the hydrochloric acid standard solution consumed in the sample, ml; V0 is the volume of the hydrochloric acid standard solution consumed in the blank sample, ml; m is the mass of the sample, g; and 45 is the molar mass of the carboxyl group, g / mol l; According to calculation, the carboxyl content in the perylene-modified nitrile rubber is 11.4%.

[0038] S2: Place 2.8 g of nano zinc oxide in 80 ml of toluene, ultrasonically disperse for 10 minutes, add 3.5 g of perylene-modified nitrile rubber, heat to 100°C, stir thoroughly for 5 hours, cool to room temperature, collect the product, and obtain an anti-ultraviolet reinforced rubber.

[0039] The acid-base titration method is used to test the carboxyl content in the UV-resistant reinforcing rubber. The specific operation method is the same as step S1. After calculation, the carboxyl content in the UV-resistant reinforcing rubber is 3.6%. Compared with the carboxyl content in the perylene-modified nitrile rubber, the carboxyl content in the UV-resistant reinforcing rubber is significantly reduced. This is due to the interaction between the carboxyl groups in the structure of the perylene-modified nitrile rubber and the hydroxyl groups on the surface of the nano zinc oxide.

[0040] 2. Preparation of flame-retardant gas gel

[0041] SS1: 2.5 g of curdlan was placed in 50 ml of deionized water, and after being fully stirred, 2.6 g of acryloyl chloride and 0.02 g of triethylamine were added, and the mixture was heated to 50 °C and stirred for 6 h. Low boiling substances were removed by vacuum distillation to obtain modified curdlan;

[0042] SS2: 3 g of modified curdlan was placed in 60 ml of N-methylpyrrolidone, 2.8 g of triallyl phosphate and 0.6 g of azobisisobutyronitrile were added, the temperature was raised to 55 °C and stirred for 8 h, low-boiling substances were removed by distillation under reduced pressure to obtain phosphorylated curdlan;

[0043] SS3: 3.5 g of phosphated curdlan was placed in 80 ml of distilled water, heated to 45°C, stirred at 300 r / min for 4 h, and solidified after freeze drying to obtain a flame-retardant gel.

[0044] The flame retardant gas gel was analyzed by scanning electron microscope S-4800 Hitach i. Figure 1 It can be seen that the flame-retardant gas gel presents a porous network structure, which can form more sound scattering and reflection interfaces, effectively improving the sound insulation effect of the sound insulation film resin.

[0045] Example 1

[0046] Preparation of sound insulation film resin

[0047] Step 1, 80 parts of polyvinyl butyral, 30 parts of anti-ultraviolet reinforcing rubber, 15 parts of flame-retardant gas gel, 5 parts of triethylene glycol diisooctanoate, and 2 parts of antioxidant 1010 are placed in a mixer and mixed thoroughly to obtain a mixture;

[0048] Step 2: Place the mixed material in a twin-screw extruder, set the screw speed to 300 r / min, the extrusion temperature to 200° C., melt-extrude and granulate to obtain a sound insulation film resin.

[0049] Example 2

[0050] Preparation of sound insulation film resin

[0051] Step 1: Place 100 parts of polyvinyl butyral, 40 parts of anti-ultraviolet reinforcing rubber, 17 parts of flame-retardant gas gel, 7 parts of triethyl citrate, and 3 parts of antioxidant 3052 in a mixer and mix them evenly to obtain a mixture;

[0052] Step 2: Place the mixed material in a twin-screw extruder, set the screw speed to 400 r / min, the extrusion temperature to 210° C., melt-extrude and granulate to obtain a sound insulation film resin.

[0053] Example 3

[0054] Preparation of sound insulation film resin

[0055] Step 1: Place 120 parts of polyvinyl butyral, 50 parts of anti-ultraviolet reinforcing rubber, 20 parts of flame-retardant gas gel, 8 parts of dibutyl sebacate, and 5 parts of antioxidant 626 in a mixer and mix them evenly to obtain a mixture;

[0056] Step 2: Place the mixed material in a twin-screw extruder, set the screw speed to 500 r / min, the extrusion temperature to 220° C., melt-extrude and granulate to obtain a sound insulation film resin.

[0057] Comparative Example 1

[0058] Preparation of sound insulation film resin

[0059] Step 1: Place 100 parts of polyvinyl butyral, 40 parts of anti-ultraviolet reinforcing rubber, 7 parts of triethyl citrate, and 3 parts of antioxidant 3052 in a mixer and mix them evenly to obtain a mixture;

[0060] Step 2: Place the mixed material in a twin-screw extruder, set the screw speed to 400 r / min, the extrusion temperature to 210° C., melt-extrude and granulate to obtain a sound insulation film resin.

[0061] Comparative Example 2

[0062] Preparation of sound insulation film resin

[0063] Step 1: Place 100 parts of polyvinyl butyral, 17 parts of flame-retardant gas gel, 7 parts of triethyl citrate, and 3 parts of antioxidant 3052 in a mixer and mix them evenly to obtain a mixture;

[0064] Step 2: Place the mixed material in a twin-screw extruder, set the screw speed to 400 r / min, the extrusion temperature to 210° C., melt-extrude and granulate to obtain a sound insulation film resin.

[0065] Comparative Example 3

[0066] Preparation of sound insulation film resin

[0067] Step 1, 100 parts of polyvinyl butyral, 40 parts of perylene-modified nitrile rubber, 17 parts of flame-retardant gas gel, 7 parts of triethyl citrate, and 3 parts of antioxidant 3052 are placed in a mixer and mixed thoroughly to obtain a mixture;

[0068] Step 2: Place the mixed material in a twin-screw extruder, set the screw speed to 400 r / min, the extrusion temperature to 210° C., melt-extrude and granulate to obtain a sound insulation film resin.

[0069] Comparative Example 4

[0070] Preparation of sound insulation film resin

[0071] Step 1, 100 parts of polyvinyl butyral, 40 parts of amino-terminated liquid nitrile rubber, 17 parts of flame-retardant gas gel, 7 parts of triethyl citrate, and 3 parts of antioxidant 3052 are placed in a mixer and mixed thoroughly to obtain a mixture;

[0072] Step 2: Place the mixed material in a twin-screw extruder, set the screw speed to 400 r / min, the extrusion temperature to 210° C., melt-extrude and granulate to obtain a sound insulation film resin.

[0073] Comparative Example 5

[0074] Preparation of sound insulation film resin

[0075] Step 1: 100 parts of polyvinyl butyral, 40 parts of anti-ultraviolet reinforcing rubber, 17 parts of curdlan, 7 parts of triethyl citrate, and 3 parts of antioxidant 3052 are placed in a mixer and mixed thoroughly to obtain a mixture;

[0076] Step 2: Place the mixed material in a twin-screw extruder, set the screw speed to 400 r / min, the extrusion temperature to 210° C., melt-extrude and granulate to obtain a sound insulation film resin.

[0077] Performance Testing

[0078] The sound insulation film resins prepared in Examples 1 to 3 and Comparative Examples 1 to 5 were made into samples that met the specifications using a universal sample preparation machine, and the sound insulation residual amount was tested using a 4206T transmission loss measuring tube. The test frequency range was 250-1600 Hz, and the sound insulation volume was tested to determine the sound insulation performance of the samples. An Instron 3365 material testing machine was used to determine the elongation at break of the samples. At the same time, the samples and the wavelength of 313 nm and the irradiance of 0.72 W / m 2 The tensile strength test of the samples after 3 days of treatment in the UV aging box was carried out to determine the mechanical strength, toughness and UV resistance of the samples; the flame retardant grade of the samples was determined according to the UL-94 standard, and the flame retardant performance of the samples was tested; the specific test results are shown in the table below:

[0079]

[0080] It can be seen from the above table that the samples prepared in Examples 1 to 3 all have excellent sound insulation, UV resistance, flame retardancy, mechanical strength and toughness, can meet the use requirements in various environments, are not easy to crack and break, and have a long service life. In the sample prepared in Comparative Example 1, no flame retardant gas gel is added, so the flame retardant performance is poor, and the sound insulation ability needs to be improved. In the sample prepared in Comparative Example 2, no anti-UV reinforcing rubber is added, the anti-UV ability is poor, the tensile strength is not high and the toughness is poor, but because the flame retardant gas gel is added, the sample has excellent flame retardant effect and sound insulation ability. In the sample prepared in Comparative Example 3, no anti-UV reinforcing rubber is added, The perylene-modified nitrile rubber was added directly, and the tensile strength and UV resistance were not as good as those in the embodiment, but since the flame-retardant gas gel was added thereto, the sound insulation effect was better and it had excellent flame retardant properties. In the sample prepared in Comparative Example 4, no UV-resistant reinforcing rubber was added, and amino-terminated liquid nitrile rubber was directly added. The UV resistance was poor, and the tensile strength was not as good as that in the embodiment, but the flame-retardant gas gel was added thereto, so the sound insulation effect and flame retardant ability were strong. In the sample prepared in Comparative Example 5, no flame-retardant gas gel was added, and curd rubber was directly added. The flame retardant effect and sound insulation ability were poor, but since the UV-resistant reinforcing rubber was added thereto, the UV resistance, tensile strength and toughness were all at a high level.

[0081] In the description of this specification, the description with reference to the terms "one embodiment", "some embodiments", "example", "specific example", or "some examples" etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representations of the above terms do not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described may be combined in any one or more embodiments or examples in a suitable manner. In addition, those skilled in the art may combine and combine the different embodiments or examples described in this specification and the features of the different embodiments or examples, without contradiction.

[0082] The above contents are merely examples and explanations of the concept of the present invention. The technicians in this technical field may make various modifications or additions to the specific embodiments described or replace them in a similar manner. As long as they do not deviate from the scope defined by the concept of the invention, they should all fall within the protection scope of the present invention.

Claims

1. An enhanced sound insulation film resin, characterized in that: The invention comprises the following raw materials in parts by weight: The anti-ultraviolet reinforcing rubber is prepared from nano zinc oxide and perylene-modified nitrile rubber; the perylene-modified nitrile rubber is prepared from amino-terminated liquid nitrile rubber and 3,4,9,10-perylenetetracarboxylic dianhydride; The flame-retardant gas gel is prepared by fully mixing phosphorylated curdlan in distilled water and solidifying it through freeze drying; the phosphorylated curdlan is prepared by modified curdlan and triallyl phosphate under the action of an initiator; the modified curdlan is prepared by curdlan and acryloyl chloride.

2. The enhanced sound insulation film resin according to claim 1, characterized in that: The plasticizer is any one of triethylene glycol diisooctanoate, triethyl citrate, dibutyl sebacate, and dioctyl phthalate; the antioxidant is any one of antioxidant 1010, antioxidant 3052, antioxidant 626, and antioxidant 1135.

3. The enhanced sound insulation film resin according to claim 1, characterized in that: The preparation method of the anti-ultraviolet reinforced rubber comprises the following steps: S1: placing the amino-terminated liquid nitrile rubber and 3,4,9,10-perylenetetracarboxylic dianhydride in a three-necked flask in a constant temperature oil bath at 65-70° C., adding N,N-dimethylformamide, stirring thoroughly for 6-8 hours, cooling to room temperature, and collecting the product to obtain perylene-modified nitrile rubber; S2: Place nano zinc oxide in toluene, disperse it by ultrasonic for 10-15 minutes, add perylene-modified nitrile rubber, heat it up with stirring, collect the product after cooling to room temperature, and obtain anti-ultraviolet reinforced rubber.

4. The enhanced sound insulation film resin according to claim 3, characterized in that: In step S1, the molecular weight of the amino-terminated liquid nitrile rubber is 9000-15000.

5. The enhanced sound insulation film resin according to claim 3, characterized in that: In step S2, the temperature of the heating and stirring is 100-108°C and the time is 5-8h.

6. The enhanced sound insulation film resin according to claim 1, characterized in that: The preparation method of the flame-retardant gas gel comprises the following steps: SS1: Place curdlan in deionized water, stir and mix thoroughly, add acryloyl chloride and catalyst, heat to 50-55°C and stir for 6-8h, remove low-boiling substances by vacuum distillation, and obtain modified curdlan; SS2: Place the modified curdlan in N-methylpyrrolidone, add triallyl phosphate and initiator, heat to 55-60°C and stir for 8-10 hours, remove low-boiling substances by distillation under reduced pressure, and obtain phosphorylated curdlan; SS3: Place the phosphated curdlan in distilled water, heat it to 45-50°C, stir it at a speed of 300-400r / min for 4-6h, solidify it after freeze-drying, and obtain a flame-retardant gel.

7. The enhanced sound insulation film resin according to claim 6, characterized in that: In step SS1, the catalyst is triethylamine.

8. The enhanced sound insulation film resin according to claim 6, characterized in that: In step SS2, the initiator is any one of azobisisobutyronitrile and azobisisoheptanenitrile.

9. A method for preparing the enhanced sound insulation film resin according to claim 1, characterized in that: The following steps are involved: Step 1: Place polyvinyl butyral, UV-resistant reinforcing rubber, flame-retardant gel, plasticizer, and antioxidant in a mixer and mix them evenly to obtain a mixture; Step 2: Place the mixed material in a twin-screw extruder, set the screw speed to 300-500 r / min, the extrusion temperature to 200-220° C., melt-extrude and granulate to obtain a sound insulation film resin.