Two-component binder for jet printing, jet printing equipment and printing method

By using two-component binders of thermally cured resin and photosensitive resin, combined with dual curing technology of ultraviolet lamp and infrared heating systems, the poor bonding effect of the middle layer to layer and the adhesive diffusion of the powder adhesive spray printing is solved. The problem of high precision and high quality printing effect is achieved.

CN119081358APending Publication Date: 2024-12-06INST OF METAL RESEARCH - CHINESE ACAD OF SCI
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411210423.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

In the existing powder adhesive jet printing technology, there are problems of poor bonding between layers, adhesive diffusion and interlayer defects, resulting in poor size and defects of printed parts.

Method used

Using a two-component binder composed of thermally cured resin and photosensitive resin, combined with dual curing technology of ultraviolet lamp and infrared heating system, each powder layer is ultraviolet cured and overall thermal cured during the printing process to improve the binder degree of curing crosslinking.

Benefits of technology

The bonding effect and shape and dimensional accuracy between layers are significantly improved, defects are reduced, and high-quality blank parts with high dimensional accuracy and defects are printed.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081358A_ABST
    Figure CN119081358A_ABST
Patent Text Reader

Abstract

The invention provides a two-component binder for jet printing, jet printing equipment and a printing method, the two-component binder comprises a component A and a component B. The component A is a thermosetting resin system, the component B is a photosensitive resin system, and the ratio of the component A to the component B in parts by mass is 1: 1-4: 1. According to the invention, each powder layer subjected to selected area spraying of the binder can be cured and crosslinked, so that the conditions of poor bonding effect between layers of the powder layers, binder diffusion, interlayer defects and the like are reduced or avoided, and the problems of poor bonding effect between layers of the powder layers, poor bonding effect between layers of the powder layers and poor bonding effect between layers of the powder binder spraying printing equipment in the prior art are solved. And even the problems of binder diffusion and interlayer defects exist, and part biscuits with high shape and size precision, few defects and high quality can be prepared through printing.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of powder materials and 3D printing, and in particular to a two-component binder for jet printing, a jet printing device and a printing method. Background Art

[0002] Additive Manufacturing (AM), also known as 3D printing or rapid prototyping, is gaining increasing attention and favor in industrial production because it can produce personalized products of various shapes compared to traditional processes. Binder Jetting (BJ) is an important AM process. This method selectively deposits the material in the powder layer by spraying a liquid binder, and heats and solidifies it to form a rough part with a certain strength. Finally, it is further densified by degreasing and sintering to obtain the final part with the required density and mechanical properties. BJ technology has the advantages of low cost, fast printing speed, high resolution and no need for support structures to achieve complex geometric shapes. These advantages have great potential for mass industrial production. BJ technology can use almost any kind of granular material and various particle sizes. In industrial production applications, it can be widely used in many fields such as automobiles, machinery, medical care, electronics, aerospace, etc., covering all aspects of people's food, clothing, housing and transportation.

[0003] Binder jetting technology is a 3D printing method based on droplet jetting and powder bonding of powder raw materials. Its core mechanism is the interaction between liquid binder and powder and their bonding force. This process determines the mechanical strength, geometric accuracy and powder removal ability of the blank. The printing process of this technology is that the powder spreading device of the equipment first spreads the powder into a flat layer, and then the print head carrying the liquid binder selectively sprays the liquid binder at the position of the desired shape, and then the powder bed drops to a layer thickness, and the "powder spreading and binder spraying" operation is repeated until the part is printed.

[0004] During the printing and powder spreading process, when the next powder layer is laid on the powder layer sprayed with binder in the selected area, the binder on the powder layer sprayed with binder is often still in a wet state, which can easily cause poor bonding effect, binder diffusion, interlayer defects and other phenomena between layers due to excessive humidity. In severe cases, it may also cause the undried binder on the surface to extend in the powder spreading direction during the powder spreading process, resulting in poor dimensional accuracy of the final printed parts and prone to defects such as cracks. On the other hand, binders with strong fluidity can continue to diffuse downward through gravity and capillary action. Especially when printing large-sized and high-height parts, the binder will continue to accumulate at the bottom of the part as the standing time increases, resulting in excessive binder at the bottom of the part and outward expansion and deformation of the part size. In addition, after the printing of the blank part is completed, the blank part needs to be taken out of the powder bed and moved into the oven for thermal curing. During the transfer process, if the binder in the blank is in an uncured state or even a wet state, the risk of defects such as blank shape deformation and internal microcracks will increase. In response to the above problems, the existing BJ equipment technology and its printing process generally set an infrared heating lamp that moves with the guide rail in front of the powder roller, and use the infrared lamp to bake the powder layer that has been sprayed with the adhesive for a short time to achieve surface curing. However, the infrared heating lamp generally cannot reach very high heat, especially for the adhesive system in which the thermal curing temperature of the curing agent is relatively high (for example, greater than 150°C). This heating lamp can only evaporate the solvent in the adhesive at most, but will not have the effect of initially curing the adhesive.

[0005] Since the powder binder jet printing equipment in the prior art has technical problems such as poor bonding between powder layers, and even binder diffusion and interlayer defects, the present invention studies and designs a two-component binder for jet printing, a jet printing equipment and a printing method. Summary of the invention

[0006] Therefore, the technical problem to be solved by the present invention is to overcome the problems of poor bonding between powder layers, poor size caused by adhesive diffusion and interlayer defects in the powder binder jet printing process in the prior art, thereby providing a two-component binder for jet printing, a jet printing device and a printing method.

[0007] In order to solve the above problems, the present invention provides a two-component adhesive for jet printing, which comprises:

[0008] Component A and component B, wherein the component A is a thermosetting resin system, the component B is a photosensitive resin system, and the ratio of the component A to the component B, in parts by mass, is component A: component B = 1:1 to 4:1.

[0009] In some embodiments,

[0010] The mass fraction of the main resin in the A component accounts for 20%-60% of the total A component, and the mass fraction of the curing agent in the A component accounts for 10%-60% of the total A component.

[0011] In some embodiments,

[0012] The main resin in the A component is an acrylic resin, specifically: one or a combination of two or more of bisphenol A epoxy acrylate, polyurethane acrylate, polyester acrylate, polyether acrylate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, octafluoropentyl methacrylate, and trifluoroethanol acrylate; and / or,

[0013] The main resin in the A component is a phenolic resin, specifically: one or a combination of two or more of cresol-formaldehyde resin, phenol-formaldehyde resin, glycerol-phenol-formaldehyde resin, and composite phenolic resin; and / or,

[0014] The main resin in the A component is at least one of polyester, polyurethane and vinyl resin.

[0015] In some embodiments,

[0016] The curing agent in the component A is a heat curing curing agent, specifically at least one of alicyclic amine curing agents, fatty amine curing agents, polythiol curing agents, aromatic amine curing agents and polyether amine curing agents.

[0017] In some embodiments,

[0018] The component A further comprises at least one of a solvent, a plasticizer, a coupling agent, a filler, a promoter, an inhibitor, an initiator and a humectant;

[0019] The mass fraction of the solvent in the A component accounts for 10%-50% of the total A component.

[0020] In some embodiments,

[0021] The mass fraction of the main resin in the B component accounts for 30%-80% of the total B component; the mass fraction of the photoinitiator in the B component accounts for 0.5%-4% of the total B component.

[0022] In some embodiments,

[0023] The main resin in the B component is an acrylic resin, specifically: one or a combination of two or more of bisphenol A epoxy acrylate, polyurethane acrylate, polyester acrylate, polyether acrylate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, octafluoropentyl methacrylate, and trifluoroethanol acrylate; and / or,

[0024] The main resin in the B component is at least one of unsaturated polyester, silicone oligomer and epoxy resin; and / or,

[0025] The photoinitiator in the component B may be one or a combination of two or more of 2-hydroxy-2-methyl-1-phenylpropanone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 1-hydroxycyclohexylbenzophenone, benzoin and its derivatives, benzil derivatives, dialkoxyacetophenone, α-hydroxyalkylbenzophenone, benzophenone and its derivatives, vinyl sulfide compounds, diazonium salts, diaryliodonium salts, triarylsulfonium salts, alkylsulfonium salts, and iron arene salts;

[0026] In some embodiments,

[0027] The B component includes, in addition to the main resin and the photoinitiator, at least one of an active diluent, a plasticizer, a defoamer, a filler, a dispersant and an inhibitor.

[0028] The present invention also provides a jet-3D printing device using the aforementioned binder, characterized in that:

[0029] The machine comprises: a frame, a powder spreading system, a negative pressure ink supply printing system, an ultraviolet lamp system, an infrared heating system, a control system, a forming cylinder system and a material cylinder system. The ultraviolet lamp system is arranged in the moving direction of the powder spreading system.

[0030] The present invention also provides a printing control method of the aforementioned jet-3D printing device, which comprises:

[0031] The powder spreading roller pushes the powder above the material cylinder to spread a layer of powder on the forming cylinder;

[0032] The adhesive printing nozzle sprays the adhesive in the set selected area, and the spraying amount and the number of spraying scans can be adjusted according to the actual situation;

[0033] The UV lamp is turned on and scanned across the molding cylinder area with the set parameters of light energy density, forward speed and number of scans to perform UV cross-linking and curing on the powder layer surface in the area where the binder is sprayed, and then the UV lamp is turned off;

[0034] The blank parts are taken out and transferred into the oven for overall heat curing at the preset temperature and holding time to finally obtain high-quality blank parts.

[0035] The two-component adhesive for jet printing, jet printing equipment and printing method provided by the present invention have the following beneficial effects:

[0036] 1. The present invention designs a two-component adhesive composed of a thermosetting resin and a photosensitive resin. When used for powder binder jet printing of part blanks, during the process of printing parts, each layer of powder layer on which the binder has been sprayed in the selected area can be cured and cross-linked, thereby reducing or avoiding the poor bonding effect between layers of the powder layer, diffusion of the binder, interlayer defects, etc., and solves the problems of poor bonding effect between layers of the powder layer, poor size caused by diffusion of the binder, and interlayer defects in the powder binder jet printing process in the prior art. In particular, the mass fraction ratio of component A to component B is 1:1 to 4:1. This binder system with thermal curing as the main component and light curing as the auxiliary component can further improve the curing and cross-linking effect of each layer of powder layer on which the binder has been sprayed in the selected area, further improve the bonding effect between layers of the powder layer and the shape and size accuracy of each layer, and thus can print and prepare high-quality blank parts with high dimensional accuracy and few defects.

[0037] 2. The present invention also increases the diversity of curing methods for printed parts by UV curing the surface of each powder layer during the printing process and overall heat curing after the part is printed; by UV curing each powder layer during the printing process, the cross-linking curing degree of the powder layer surface is improved, thereby avoiding defects between adjacent powder layers and poor dimensional accuracy of the final part blank due to uncured adhesive on the surface of the powder layer sprayed in the selected area; the present invention also further improves the part blank with UV cured surface of each powder layer through the process of overall heat curing after the blank part is taken out of the powder bed and moved into an oven, so that the blank part has better interlayer strength, and further avoids the occurrence of defects such as internal cracks in the part caused by the movement of the part during the transfer process. BRIEF DESCRIPTION OF THE DRAWINGS

[0038] Figure 1 is a top view of the binder jetting-3D printing apparatus of the present invention;

[0039] Figure 2 is a front view of the binder jetting-3D printing device of the present invention.

[0040] The reference numerals are as follows:

[0041] 1. Guide rail; 2. UV curing lamp; 3. Print nozzle; 4. Powder roller; 5. Infrared heating lamp; 6. Moving parts; 7. Material cylinder; 8. Forming cylinder; 9. Equipment table; 10. Raw material powder; 11. Adhesive spray printing area; 12. Negative pressure ink supply circulation system; 13. Motor control and belt conveyor system; 14. The sinking part of the part; 15. Powder bed. DETAILED DESCRIPTION

[0042] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, rather than all the embodiments. The following description of at least one exemplary embodiment is actually only illustrative and is by no means intended to limit the present invention and its application or use. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0043] It should be noted that the terms used herein are only for describing specific embodiments and are not intended to limit the exemplary embodiments according to the present application. As used herein, unless the context clearly indicates otherwise, the singular form is also intended to include the plural form. In addition, it should be understood that when the terms "comprise" and / or "include" are used in this specification, it indicates the presence of features, steps, operations, devices, components and / or combinations thereof.

[0044] Unless otherwise specifically stated, the relative arrangement of the parts and steps described in these embodiments, numerical expressions and numerical values ​​do not limit the scope of the present invention. At the same time, it should be understood that, for ease of description, the sizes of the various parts shown in the accompanying drawings are not drawn according to the actual proportional relationship. The technology, method and equipment known to ordinary technicians in the relevant field may not be discussed in detail, but in appropriate cases, the technology, method and equipment should be regarded as a part of the authorization specification. In all examples shown and discussed here, any specific value should be interpreted as being merely exemplary, rather than as a limitation. Therefore, other examples of exemplary embodiments may have different values. It should be noted that similar reference numerals and letters represent similar items in the following drawings, so once a certain item is defined in an accompanying drawing, it does not need to be further discussed in subsequent drawings.

[0045] In the description of the present invention, it is necessary to understand that the directions or positional relationships indicated by directional words such as "front, back, up, down, left, right", "lateral, vertical, perpendicular, horizontal" and "top, bottom" are usually based on the directions or positional relationships shown in the drawings. They are only for the convenience of describing the present invention and simplifying the description. Unless otherwise specified, these directional words do not indicate or imply that the devices or elements referred to must have a specific direction or be constructed and operated in a specific direction. Therefore, they cannot be understood as limiting the scope of protection of the present invention. The directional words "inside and outside" refer to the inside and outside relative to the contours of each component itself.

[0046] For ease of description, spatially relative terms such as "above", "above", "on the upper surface of", "above", etc. may be used here to describe the spatial positional relationship between a device or feature and other devices or features as shown in the figure. It should be understood that spatially relative terms are intended to include different orientations of the device in use or operation in addition to the orientation described in the figure. For example, if the device in the accompanying drawings is inverted, the device described as "above other devices or structures" or "above other devices or structures" will be positioned as "below other devices or structures" or "below other devices or structures". Thus, the exemplary term "above" can include both "above" and "below". The device can also be positioned in other different ways (rotated 90 degrees or in other orientations), and the spatially relative descriptions used here are interpreted accordingly.

[0047] In addition, it should be noted that the use of terms such as "first" and "second" to limit components is only for the convenience of distinguishing the corresponding components. If not otherwise stated, the above terms have no special meaning and therefore cannot be understood as limiting the scope of protection of the present invention.

[0048] like Figure 1-2 As shown, the present invention provides a two-component binder for jet printing (preferably a two-component binder for powder binder jet printing), which comprises:

[0049] Component A and component B, wherein the component A is a thermosetting resin system, the component B is a photosensitive resin system, and the ratio of the component A to the component B, in parts by mass, is component A: component B = 1:1-4:1, preferably, component A: component B = 2:1-3:1.

[0050] The present invention designs a two-component adhesive composed of a thermosetting resin and a photosensitive resin. When used for powder binder jet printing of a blank part, during the process of printing the part, each layer of powder on which the binder has been jetted in a selected area can be cured and cross-linked, thereby reducing or avoiding the poor bonding effect between layers of the powder layer, the diffusion of the binder, the defects between layers, and the like. The present invention solves the problem that the powder binder jet printing equipment in the prior art has a poor bonding effect between layers of the powder layer, and even the diffusion of the binder and the defects between layers. In particular, the mass fraction ratio of the A component to the B component is 1:1 to 4:1, which can further improve the curing and cross-linking effect of each layer of powder on which the binder has been jetted in a selected area, further improve the bonding effect between layers of the powder layer, and thus print and prepare high-quality blank parts with high dimensional accuracy and few defects.

[0051] In some embodiments,

[0052] The mass fraction (wt%) of the main resin in the A component accounts for 20%-60% of the total A component, and the mass fraction (wt%) of the curing agent in the A component accounts for 10%-60% of the total A component.

[0053] In some embodiments,

[0054] The main resin in the A component is an acrylic resin, specifically: one or a combination of two or more of bisphenol A epoxy acrylate, polyurethane acrylate, polyester acrylate, polyether acrylate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, octafluoropentyl methacrylate, and trifluoroethanol acrylate; and / or,

[0055] The main resin in the A component is a phenolic resin, specifically: one or a combination of two or more of cresol-formaldehyde resin, phenol-formaldehyde resin, glycerol-phenol-formaldehyde resin, and composite phenolic resin; and / or,

[0056] The main resin in the A component is at least one of polyester, polyurethane and vinyl resin.

[0057] In some embodiments,

[0058] The curing agent in the component A is a heat curing curing agent, specifically at least one of alicyclic amine curing agents, fatty amine curing agents, polythiol curing agents, aromatic amine curing agents and polyether amine curing agents.

[0059] In some embodiments,

[0060] The component A further comprises at least one of a solvent, a plasticizer, a coupling agent, a filler, a promoter, an inhibitor, an initiator and a humectant;

[0061] The mass fraction of the solvent in the A component accounts for 10%-50% of the total A component, preferably, 10%-30% of the total A component.

[0062] In some embodiments,

[0063] The mass fraction of the main resin in the B component accounts for 30%-80% of the total B component; the mass fraction of the photoinitiator in the B component accounts for 0.5%-4% of the total B component, preferably, 1%-2% of the total B component.

[0064] When the amount of photoinitiator is insufficient, the free radical density in the binder is insufficient, which will make the UV-curing cross-linking degree of the binder on the surface of the powder layer insufficient, and the powder layer cannot be initially cured; when the amount of photoinitiator in the formula is excessive, too many free radicals will make the curing cross-linking degree of the powder layer surface too high, making the powder layer surface too hard, which will increase the brittleness of the powder layer, and make it easy for the surface powder layer after UV curing and the deep powder layer that has not been UV cured to be squeezed and deformed, which is not conducive to the effect of the subsequent thermal curing process.

[0065] In some embodiments,

[0066] The main resin in the B component is an acrylic resin, specifically: one or a combination of two or more of bisphenol A epoxy acrylate, polyurethane acrylate, polyester acrylate, polyether acrylate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, octafluoropentyl methacrylate, and trifluoroethanol acrylate; and / or,

[0067] The main resin in the B component is at least one of unsaturated polyester, silicone oligomer and epoxy resin; and / or,

[0068] The photoinitiator in the component B may be one or a combination of two or more of 2-hydroxy-2-methyl-1-phenylpropanone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 1-hydroxycyclohexylbenzophenone, benzoin and its derivatives, benzil derivatives, dialkoxyacetophenone, α-hydroxyalkylbenzophenone, benzophenone and its derivatives, vinyl sulfide compounds, diazonium salts, diaryliodonium salts, triarylsulfonium salts, alkylsulfonium salts, and iron arene salts;

[0069] In some embodiments,

[0070] The B component includes, in addition to the main resin and the photoinitiator, at least one of an active diluent, a plasticizer, a defoamer, a filler, a dispersant and an inhibitor.

[0071] Furthermore, the main resins in the A component and the B component of the binder system may be the same resin component or different resin components, but are preferably the same resin component.

[0072] The present invention also provides a jet-3D printing device using the aforementioned binder, which includes: a frame, a powder spreading system, a negative pressure ink supply printing system, an ultraviolet lamp system, an infrared heating system, a control system, a molding cylinder system and a material cylinder system, wherein the ultraviolet lamp system is arranged in the direction of movement of the powder spreading system.

[0073] The present invention also increases the diversity of curing methods for printed parts by UV curing the surface of each powder layer during the printing process and overall heat curing after the part is printed; by UV curing each powder layer during the printing process, the cross-linking curing degree of the powder layer surface is improved, avoiding defects between adjacent powder layers and poor dimensional accuracy of the final part blank caused by uncured adhesive on the surface of the powder layer sprayed in the selected area.

[0074] The binder jetting-3D printing device of the present invention has moving parts integrated on the horizontal guide rail, including a UV curing lamp, a print nozzle, a powder spreading roller and an infrared heating lamp. The moving parts are arranged along the advancing direction of the horizontal guide rail, as shown in the accompanying drawings. Figure 1 and Figure 2 As shown, they are, in sequence, an infrared heating lamp, a powder spreading roller, a printing nozzle, and a UV curing lamp.

[0075] The present invention provides a two-component adhesive for powder adhesive jet printing, a BJ device capable of printing and preparing blank parts with high dimensional accuracy and few defects, and a binder jet printing molding process method for preparing blank parts with high dimensional accuracy and few defects. The main purpose is to improve the cross-linking and curing degree of the powder layer surface by ultraviolet curing of each powder layer during the printing of the blank parts, thereby avoiding the phenomenon that defects are easily generated between adjacent powder layers in the printing area (adhesive jet printing area 11) due to the binder on the surface of the powder layer sprayed in the selected area not yet cross-linked and cured, thereby being able to print and prepare high-quality blank parts with high dimensional accuracy and few defects.

[0076] In one embodiment of the present invention, the binder jetting-3D printing equipment described above is used, and the printing material is powdered Si3N4 (α phase>90%) and the particle size is graded. The specific grading is calculated by mass fraction (wt%): 0.8μm (D50) 30%, 25μm (D50) 40%, 60μm (D50) 30%.

[0077] The blank shape of the printed parts is a sample strip of 80mm×35mm×20mm.

[0078] The adhesive used is a homemade two-component adhesive, in which component A includes bisphenol A epoxy acrylate (main resin), modified alicyclic amine curing agent, propylene oxide butyl ether (solvent), phthalate (plasticizer), KH560 (coupling agent) and other additives; component B includes bisphenol A epoxy acrylate (main resin), propylene oxide butyl ether (active diluent), 2,4,6-trimethylbenzoyldiphenylphosphine oxide (photoinitiator) and other additives.

[0079] During the printing process, the thickness of a single powder layer is 0.1 mm, the reference voltage of the negative pressure inkjet system is set to 60 V, the UV light source is a high-pressure mercury lamp, the vertical distance between the UV light source and the powder bed 15 is 15 cm, and the UV light source scans the forming cylinder twice; after the printing of the parts is completed, the part blank is taken out and placed in an oven for curing at 150°C for 2 hours, and then taken out to obtain a high-quality part blank.

[0080] Evaluation criteria for blank part performance: In a feasible implementation plan, the dimensional accuracy error must be less than ±0.50mm, and the flexural strength must be greater than 5MPa (the significant increase in flexural strength reflects that the bonding effect between the powder layers is effectively enhanced).

[0081] Furthermore, the components of the ultraviolet lamp system at least include a UV light source, a reflecting device, and a cooling device.

[0082] Specifically, the UV light source can be one of a high-pressure mercury lamp, an electrodeless lamp, and a UV-LED lamp tube. The wavelength of the UV light source is 200nm-420nm, and the preferred main wavelength is 365nm.

[0083] Specifically, the distance between the UV light source and the plane of the powder bed 15 is 10 cm to 25 cm, preferably 15 cm to 20 cm.

[0084] Specifically, the light energy density of the UV light source is adjustable within the range of 0-2000 MJ / cm2.

[0085] Specifically, the role of the ultraviolet lamp system is to accelerate the curing and cross-linking of the surface of the powder layer after the binder is sprayed on the powder layer, so as to avoid the poor bonding effect, adhesive diffusion, interlayer defects and the like caused by excessive humidity between layers, thereby further improving the dimensional accuracy of the final printed parts and reducing the incidence of defects in the parts.

[0086] Furthermore, the binder jetting-3D printing device, whose moving parts integrated on the horizontal guide rail (guide rail 1) include at least a UV curing lamp 2, a print nozzle 3, and a powder spreading roller 4. Preferably, the moving parts include a UV curing lamp 2, a print nozzle 3, a powder spreading roller 4 and an infrared heating lamp 5.

[0087] Specifically, the frame of the 3D printing device can be designed in an integrated manner according to actual application requirements and the work frame, and the material is preferably an aluminum alloy frame.

[0088] Specifically, the powder spreading system of the 3D printing device is mainly composed of a linear guide rail, a powder spreading roller, a servo motor, etc., and its function is to evenly spread the special powder used for molding onto the molding plane.

[0089] Specifically, the molding cylinder system of the 3D printing device mainly includes a cylinder body, a piston, a guide rod, a servo motor and the like.

[0090] Specifically, the cylinder system of the 3D printing device mainly includes a cylinder body, a piston, a guide rod, a servo motor and the like.

[0091] Specifically, the negative pressure ink supply printing system of the 3D printing device mainly includes a print head and an ink supply circulation system. The ink supply circulation system mainly includes a main ink barrel, a negative pressure air pipe, an ink tube, an auxiliary ink cartridge, a control board, etc. Its function is to provide circulating adhesive for the inkjet printing system and the print head sprays a set amount of adhesive according to the program setting.

[0092] Specifically, the control system of the 3D printing equipment is a system with a computer as the core, which controls the nozzle to select inkjet printing on the surface of the powder bed and realizes the layer-by-layer superposition of the printing area by mechanical and electrical means. It is mainly composed of an electrical control box, an industrial computer, a PLC and other auxiliary components.

[0093] Specifically, the binder jetting-3D printing device, in addition to the components described above, may also include components such as a cleaning system, a moisturizing system, and a powder recovery system according to actual application requirements and scenarios.

[0094] The attached drawings of the present invention are a feasible implementation within the scope of patent protection, wherein the infrared heating lamp 5 may or may not be present, and the UV curing lamp 2 is a necessary component, and the position may be at the leftmost end or the rightmost end of the moving component part.

[0095] The present invention also provides a printing control method of the aforementioned jet-3D printing device, which comprises:

[0096] The powder spreading roller pushes the powder above the material cylinder 11 to spread a powder layer on the forming cylinder 8;

[0097] The adhesive printing nozzle sprays the adhesive in the set selected area, and the spraying amount and the number of spraying scans can be adjusted according to the actual situation;

[0098] The UV lamp is turned on and scanned across the molding cylinder area with the set parameters of light energy density, forward speed and number of scans to perform UV cross-linking and curing on the powder layer surface in the area where the binder is sprayed, and then the UV lamp is turned off;

[0099] The blank parts are taken out and transferred into the oven for overall heat curing at the preset temperature and holding time to finally obtain high-quality blank parts.

[0100] The present invention provides a specific printing method and steps for powder binder jet printing of high-strength blanks, wherein the key or special steps mainly include: feeding and powder spreading operations, printing parts according to processing files, selective area binder jetting, ultraviolet curing of the binder on the surface of the powder layer, and curing of the blanks of the parts in an oven.

[0101] The present invention also increases the diversity of curing methods for printed parts by UV curing the surface of each powder layer during the printing process and overall heat curing after the part is printed; by UV curing each powder layer during the printing process, the cross-linking curing degree of the powder layer surface is improved, thereby avoiding defects between adjacent powder layers and poor dimensional accuracy of the final part blank due to uncured adhesive on the surface of the powder layer sprayed in the selected area; the present invention also further improves the part blank with UV cured surface of each powder layer through the process of overall heat curing after the blank part is taken out of the powder bed and moved into an oven, so that the part blank has better interlayer strength, and further avoids the occurrence of defects such as internal cracks in the part caused by the movement of the part during the transfer process.

[0102] Specifically, the present invention provides a method for preparing high-quality green blanks by powder binder jet printing, and the specific steps mainly include:

[0103] (1) Design the 3D model of the part to be printed, select the printing material, set the layer thickness, and slice it to generate a .cli file according to actual needs;

[0104] (2) Power on the printing device, run the negative pressure inkjet system, and then return all axes of the device to zero;

[0105] (3) Loading and powder spreading operation: lower the height of the material cylinder from the highest limit to a certain height (according to the height of the printed part), pour the raw material powder into the material cylinder, set the powder spreading parameters and start the powder spreading operation until the surface of the forming cylinder is flattened;

[0106] (4) Import the processing file (.cli slice file) into the device computer and set the appropriate printing parameters and UV lamp curing parameters;

[0107] (5) Start the printing operation. The guide rail on the equipment platform starts to move. Follow the following steps in sequence according to the parameters set in the program:

[0108] ① The powder spreading roller pushes the powder above the material cylinder to spread a layer of powder on the forming cylinder.

[0109] ② The adhesive printing nozzle sprays the adhesive in the set selected area. The spraying amount and the number of spraying scans can be adjusted according to the actual situation.

[0110] ③ The UV lamp is turned on and scanned across the molding cylinder area with the set parameters such as light energy density, forward speed and number of scans to perform UV cross-linking and curing on the powder layer surface in the area where the binder has just been sprayed, and then the UV lamp is turned off.

[0111] ④After that, the above components return to the coordinate zero point along with the guide rail, and then continue to repeat the above steps ①-③ until the printing program is completed.

[0112] (6) The blank is taken out and placed in an oven for heat curing at a certain temperature and insulation time to obtain high-quality blank parts.

[0113] Specifically, during the printing process, the light energy density of the UV light source is preferably 500-1500 MJ / cm 2 ,

[0114] Specifically, during the printing process, the forward speed of the UV light source can be set to 0.5 cm / s-8 cm / s, preferably 1 cm / s-4 cm / s.

[0115] Specifically, during the printing process, the UV light source may scan the molding cylinder area 1 to 4 times, preferably 2 times.

[0116] Specifically, the adhesive used in the printing implementation process is the two-component adhesive described in the first aspect.

[0117] Specifically, the raw material powder can be powder of various materials, specifically metal powder, ceramic powder, alloy powder, or special powder with different particle size distribution or mixed with different materials.

[0118] Specifically, the raw material powder is preferably a spherical powder, because after the spherical powder is spread into a powder layer, it is easier for ultraviolet light to penetrate deeper into the powder layer.

[0119] Specifically, the particle size of the raw material powder is 0.5 μm-200 μm, preferably 10 μm-80 μm, and more preferably a powder obtained by grading fine particle powder of 0.5 μm-10 μm and coarser particle powder of 10 μm-100 μm.

[0120] Specifically, the raw material powder should avoid using powder with lamellar morphology and a particle size greater than 80 μm as much as possible, because such powder will reduce the ability of ultraviolet light to penetrate the powder layer, making it difficult to penetrate a thicker powder layer.

[0121] Specifically, during the printing process, it is necessary to set the preferred printing parameters such as powder layer thickness and UV curing parameters according to the material, particle size, morphology and other characteristics of the specific raw material powder, so as to finally prepare a high-quality part blank.

[0122] Example 1

[0123] The adhesive used is a self-made two-component adhesive, and the A component / B component is 2:1 in terms of weight fraction (wt%). The A component (weight fraction, wt%) includes 40% of bisphenol A epoxy acrylate (main resin), 25% of modified alicyclic amine curing agent, 30% of propylene oxide butyl ether (solvent), 1% of phthalate (plasticizer), 1% of KH560 (coupling agent), and 3% of other additives; the B component includes 60% of bisphenol A epoxy acrylate (main resin), 35% of propylene oxide butyl ether (active diluent), 1% of 2,4,6-trimethylbenzoyl diphenylphosphine oxide (photoinitiator), and 4% of other additives.

[0124] The UV curing parameters during the printing process are: UV light source energy density 1000MJ / cm 2 , the forward speed of the UV light source is 3cm / s.

[0125] The final blank of the part has a dimensional accuracy error of ±0.15mm and a bending strength of 10.4MPa.

[0126] Example 2

[0127] The adhesive used is a self-made two-component adhesive, and the A component / B component is 3:1 in terms of weight fraction (wt%). The A component (weight fraction, wt%) includes 40% of bisphenol A epoxy acrylate (main resin), 25% of modified alicyclic amine curing agent, 30% of propylene oxide butyl ether (solvent), 1% of phthalate (plasticizer), 1% of KH560 (coupling agent), and 3% of other additives; the B component includes 60% of bisphenol A epoxy acrylate (main resin), 35% of propylene oxide butyl ether (active diluent), 1% of 2,4,6-trimethylbenzoyl diphenylphosphine oxide (photoinitiator), and 4% of other additives.

[0128] The UV curing parameters during the printing process are: UV light source energy density 1000MJ / cm 2 , the forward speed of the UV light source is 3cm / s.

[0129] The final blank of the part has a dimensional accuracy error of ±0.30mm and a bending strength of 8.0MPa.

[0130] Example 3

[0131] The adhesive used is a self-made two-component adhesive, and the A component / B component is 2:1 in terms of weight fraction (wt%). The A component (weight fraction, wt%) includes 35% of bisphenol A epoxy acrylate (main resin), 35% of modified alicyclic amine curing agent, 25% of propylene oxide butyl ether (solvent), 1% of phthalate (plasticizer), 1% of KH560 (coupling agent), and 3% of other additives; the B component includes 60% of bisphenol A epoxy acrylate (main resin), 35% of propylene oxide butyl ether (active diluent), 1% of 2,4,6-trimethylbenzoyl diphenylphosphine oxide (photoinitiator), and 4% of other additives.

[0132] The UV curing parameters during the printing process are: UV light source energy density 1000MJ / cm 2 , the forward speed of the UV light source is 3cm / s.

[0133] The final blank of the part has a dimensional accuracy error of ±0.25mm and a bending strength of 9.3MPa.

[0134] Example 4

[0135] The adhesive used is a self-made two-component adhesive, and the A component / B component is 2:1 in terms of weight fraction (wt%). The A component (weight fraction, wt%) includes 40% of bisphenol A epoxy acrylate (main resin), 25% of modified alicyclic amine curing agent, 30% of propylene oxide butyl ether (solvent), 1% of phthalate (plasticizer), 1% of KH560 (coupling agent), and 3% of other additives; the B component includes 70% of bisphenol A epoxy acrylate (main resin), 25% of propylene oxide butyl ether (active diluent), 1% of 2,4,6-trimethylbenzoyl diphenylphosphine oxide (photoinitiator), and 4% of other additives.

[0136] The UV curing parameters during the printing process are: UV light source energy density 1000MJ / cm 2 , the forward speed of the UV light source is 3cm / s.

[0137] The final blank of the part has a dimensional accuracy error of ±0.25mm and a bending strength of 8.8MPa.

[0138] Example 5

[0139] The adhesive used is a self-made two-component adhesive, and the A component / B component is 2:1 in terms of weight fraction (wt%). The A component (weight fraction, wt%) includes 50% of bisphenol A epoxy acrylate (main resin), 30% of modified alicyclic amine curing agent, 15% of propylene oxide butyl ether (solvent), 1% of phthalate (plasticizer), 1% of KH560 (coupling agent), and 3% of other additives; the B component includes 50% of bisphenol A epoxy acrylate (main resin), 45% of propylene oxide butyl ether (active diluent), 1% of 2,4,6-trimethylbenzoyl diphenylphosphine oxide (photoinitiator), and 4% of other additives.

[0140] The UV curing parameters during the printing process are: UV light source energy density 1000MJ / cm 2 , the forward speed of the UV light source is 3cm / s.

[0141] The final blank of the part has a dimensional accuracy error of ±0.30mm and a bending strength of 8.3MPa.

[0142] Example 6

[0143] The adhesive used is a self-made two-component adhesive, and the A component / B component is 2:1 in terms of weight fraction (wt%). The A component (weight fraction, wt%) includes 40% of bisphenol A epoxy acrylate (main resin), 25% of modified alicyclic amine curing agent, 30% of propylene oxide butyl ether (solvent), 1% of phthalate (plasticizer), 1% of KH560 (coupling agent), and 3% of other additives; the B component includes 60% of bisphenol A epoxy acrylate (main resin), 35% of propylene oxide butyl ether (active diluent), 1% of 2,4,6-trimethylbenzoyl diphenylphosphine oxide (photoinitiator), and 4% of other additives.

[0144] The UV curing parameters during the printing process are: UV light source energy density 1500MJ / cm 2 , the forward speed of the UV light source is 5cm / s.

[0145] The final blank of the part has a dimensional accuracy error of ±0.30mm and a bending strength of 7.8MPa.

[0146] Example 7

[0147] The adhesive used is a self-made two-component adhesive, and the A component / B component is 2:1 in terms of weight fraction (wt%). The A component (weight fraction, wt%) includes 40% of bisphenol A epoxy acrylate (main resin), 25% of modified alicyclic amine curing agent, 30% of propylene oxide butyl ether (solvent), 1% of phthalate (plasticizer), 1% of KH560 (coupling agent), and 3% of other additives; the B component includes 60% of bisphenol A epoxy acrylate (main resin), 35% of propylene oxide butyl ether (active diluent), 1% of 2,4,6-trimethylbenzoyl diphenylphosphine oxide (photoinitiator), and 4% of other additives.

[0148] The UV curing parameters during the printing process are: UV light source energy density 500MJ / cm 2 , the forward speed of the UV light source is 1cm / s.

[0149] The final blank of the part has a dimensional accuracy error of ±0.25mm and a bending strength of 8.9MPa.

[0150] Comparative Example 1

[0151] The adhesive used is a self-made two-component adhesive, and the ratio of component A to component B is 2:1 by weight. Component A (by weight, wt%) includes 25% of bisphenol A epoxy acrylate (main resin), 15% of modified alicyclic amine curing agent, 55% of propylene oxide butyl ether (solvent), 1% of phthalate (plasticizer), 1% of KH560 (coupling agent), and 3% of other additives; component B includes 60% of bisphenol A epoxy acrylate (main resin), 35% of propylene oxide butyl ether (active diluent), 1% of 2,4,6-trimethylbenzoyl diphenylphosphine oxide (photoinitiator), and 4% of other additives.

[0152] The UV curing parameters during the printing process are: UV light source energy density 1000MJ / cm 2 , the forward speed of the UV light source is 3cm / s.

[0153] The final blank of the part has a dimensional accuracy error of ±0.90mm and a bending strength of 5.3MPa.

[0154] Note: When the mass percentage of the solvent in component A of the binder is too high, it will affect the printing accuracy of the binder jetting process, thereby affecting the dimensional accuracy and bending strength of the final part blank.

[0155] Comparative Example 2

[0156] The adhesive used is a self-made two-component adhesive, and the A component / B component is 2:1 in terms of weight fraction (wt%). The A component (weight fraction, wt%) includes 40% of bisphenol A epoxy acrylate (main resin), 25% of modified alicyclic amine curing agent, 30% of propylene oxide butyl ether (solvent), 1% of phthalate (plasticizer), 1% of KH560 (coupling agent), and 3% of other additives; the B component includes 58% of bisphenol A epoxy acrylate (main resin), 34% of propylene oxide butyl ether (active diluent), 4% of 2,4,6-trimethylbenzoyl diphenylphosphine oxide (photoinitiator), and 4% of other additives.

[0157] The UV curing parameters during the printing process are: UV light source energy density 1000MJ / cm 2 , the forward speed of the UV light source is 3cm / s.

[0158] The final blank of the part has a dimensional accuracy error of ±0.70mm and a bending strength of 4.6MPa.

[0159] Note: When the photoinitiator in the B component of the binder is excessive, too many free radicals will make the curing and cross-linking degree of the powder layer surface too high, making the powder layer surface too hard and increasing the brittleness of the powder layer, making it easy to cause extrusion deformation between the UV-cured surface powder layer and the deep powder layer that has not been UV-cured, which is not conducive to the effect of the subsequent thermal curing process. This will further affect the dimensional accuracy and bending strength of the final part blank.

[0160] Comparative Example 3

[0161] The adhesive used is a self-made two-component adhesive, and the ratio of component A to component B is 0.8:1 by weight. Component A (by weight, wt%) includes 40% of bisphenol A epoxy acrylate (main resin), 25% of modified alicyclic amine curing agent, 30% of propylene oxide butyl ether (solvent), 1% of phthalate (plasticizer), 1% of KH560 (coupling agent), and 3% of other additives; component B includes 60% of bisphenol A epoxy acrylate (main resin), 35% of propylene oxide butyl ether (active diluent), 1% of 2,4,6-trimethylbenzoyl diphenylphosphine oxide (photoinitiator), and 4% of other additives.

[0162] The UV curing parameters during the printing process are: UV light source energy density 1000MJ / cm 2 , the forward speed of the UV light source is 3cm / s.

[0163] The final blank of the part has a dimensional accuracy error of ±0.80mm and a bending strength of 3.3MPa.

[0164] Note: When the mass percentage (wt%) of component A / component B in the binder formula is less than 1, it will affect the thermal curing effect of the blank part, resulting in poor bending strength of the blank part; and too much photosensitive resin during the printing process will also cause the degree of curing and cross-linking of the powder layer to be too high, thereby reducing the dimensional accuracy of the part.

[0165] Comparative Example 4

[0166] The adhesive used is a self-made two-component adhesive, and the ratio of component A to component B is 4.2:1 by weight. Component A (by weight, wt%) includes 40% of bisphenol A epoxy acrylate (main resin), 25% of modified alicyclic amine curing agent, 30% of propylene oxide butyl ether (solvent), 1% of phthalate (plasticizer), 1% of KH560 (coupling agent), and 3% of other additives; component B includes 60% of bisphenol A epoxy acrylate (main resin), 35% of propylene oxide butyl ether (active diluent), 1% of 2,4,6-trimethylbenzoyl diphenylphosphine oxide (photoinitiator), and 4% of other additives.

[0167] The UV curing parameters during the printing process are: UV light source energy density 1000MJ / cm 2 , the forward speed of the UV light source is 3cm / s.

[0168] The final blank of the part has a dimensional accuracy error of ±1.3mm and a bending strength of 7.3MPa.

[0169] Note: When the mass fraction (wt%) of component A / component B in the binder formula is greater than 4, the binder on the surface of the powder layer will not be cross-linked and cured sufficiently during the printing process, thus affecting the dimensional accuracy of the final part blank.

[0170] Comparative Example 5

[0171] The adhesive used is a self-made two-component adhesive, and the A component / B component is 2:1 in terms of weight fraction (wt%). The A component (weight fraction, wt%) includes 40% of bisphenol A epoxy acrylate (main resin), 25% of modified alicyclic amine curing agent, 30% of propylene oxide butyl ether (solvent), 1% of phthalate (plasticizer), 1% of KH560 (coupling agent), and 3% of other additives; the B component includes 60% of bisphenol A epoxy acrylate (main resin), 35% of propylene oxide butyl ether (active diluent), 1% of 2,4,6-trimethylbenzoyl diphenylphosphine oxide (photoinitiator), and 4% of other additives.

[0172] The UV curing parameters during the printing process are: UV light source energy density 300MJ / cm 2 , the forward speed of the UV light source is 5cm / s.

[0173] The final blank of the part has a dimensional accuracy error of ±1.2mm and a bending strength of 6.8MPa.

[0174] Note: When the light energy density of the UV light source is low and the forward speed is fast, the binder on the surface of the powder layer will not be cross-linked and cured sufficiently during the printing process, thus affecting the dimensional accuracy of the final part blank.

[0175] Comparative Example 6

[0176] The adhesive used is a self-made two-component adhesive, and the A component / B component is 2:1 in terms of weight fraction (wt%). The A component (weight fraction, wt%) includes 40% of bisphenol A epoxy acrylate (main resin), 25% of modified alicyclic amine curing agent, 30% of propylene oxide butyl ether (solvent), 1% of phthalate (plasticizer), 1% of KH560 (coupling agent), and 3% of other additives; the B component includes 60% of bisphenol A epoxy acrylate (main resin), 35% of propylene oxide butyl ether (active diluent), 1% of 2,4,6-trimethylbenzoyl diphenylphosphine oxide (photoinitiator), and 4% of other additives.

[0177] The UV curing parameters during the printing process are: UV light source energy density 2000MJ / cm 2 , the forward speed of the UV light source is 0.5cm / s.

[0178] The final blank of the part has a dimensional accuracy error of ±0.70mm and a bending strength of 4.4MPa.

[0179] Note: When the light energy density of the UV light source is high and the forward speed is slow, the degree of curing and cross-linking of the powder layer during the printing process will be too high, thereby reducing the dimensional accuracy of the parts.

[0180] The feasible binder example formulas listed in the present invention and the binder comparative formulas that do not conform to the patent invention are shown in Table 1 below:

[0181] Table 1

[0182]

[0183] Note: Adhesive Nos. 1-5 are feasible examples of adhesive formulations, and adhesive Nos. 6-9 are comparative examples of adhesive formulations.

[0184] The values ​​and results of the printing parameters and the conditions of the part blanks prepared by printing in Examples 1-7 and Comparative Examples 1-6 listed in the present invention are shown in Table 2 below:

[0185] Table 2

[0186]

[0187]

[0188] The above examples are only partial application examples of the present invention, but the present invention is not limited to the embodiments. As long as the technical effects of the present invention are achieved by any same or similar methods or process flows, they should fall within the protection scope of the present invention.

[0189] The above is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions and improvements made within the spirit and principles of the present invention shall be included in the protection scope of the present invention. The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and variations can be made without departing from the technical principles of the present invention. Any combination of the embodiments shall also be regarded as the protection scope of the present invention.

Claims

1. A two-component adhesive for jet printing, Features: include: Component A and component B, wherein the component A is a thermosetting resin system, the component B is a photosensitive resin system, and the ratio of the component A to the component B, in parts by mass, is component A: component B = 1:1-4:

1.

2. The two-component adhesive for jet printing according to claim 1, Features: The mass fraction of the main resin in the A component accounts for 20%-60% of the total A component, and the mass fraction of the curing agent in the A component accounts for 10%-60% of the total A component.

3. The two-component adhesive for jet printing according to claim 2, Features: The main resin in the A component is an acrylic resin, specifically: one or a combination of two or more of bisphenol A epoxy acrylate, polyurethane acrylate, polyester acrylate, polyether acrylate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, octafluoropentyl methacrylate, and trifluoroethanol acrylate; and / or, The main resin in the A component is a phenolic resin, specifically: one or a combination of two or more of cresol-formaldehyde resin, phenol-formaldehyde resin, glycerol-phenol-formaldehyde resin, and composite phenolic resin; and / or, The main resin in the A component is at least one of polyester, polyurethane and vinyl resin.

4. The two-component adhesive for jet printing according to claim 2, Features: The curing agent in the component A is a heat curing curing agent, specifically at least one of alicyclic amine curing agents, fatty amine curing agents, polythiol curing agents, aromatic amine curing agents and polyether amine curing agents.

5. The two-component adhesive for jet printing according to claim 2, Features: The component A further comprises at least one of a solvent, a plasticizer, a coupling agent, a filler, a promoter, an inhibitor, an initiator and a humectant; The mass fraction of the solvent in the A component accounts for 10%-50% of the total A component.

6. The two-component adhesive for jet printing according to claim 1, Features: The mass fraction of the main resin in the B component accounts for 30%-80% of the total B component; the mass fraction of the photoinitiator in the B component accounts for 0.5%-4% of the total B component.

7. The two-component adhesive for jet printing according to claim 6, Features: The main resin in the B component is an acrylic resin, specifically: one or a combination of two or more of bisphenol A epoxy acrylate, polyurethane acrylate, polyester acrylate, polyether acrylate, tripropylene glycol diacrylate, 1,6-hexanediol diacrylate, octafluoropentyl methacrylate, and trifluoroethanol acrylate; and / or, The main resin in the B component is at least one of unsaturated polyester, silicone oligomer and epoxy resin; and / or, The photoinitiator in the component B can be one or a combination of two or more of 2-hydroxy-2-methyl-1-phenylpropanone, 2,4,6-trimethylbenzoyldiphenylphosphine oxide, 1-hydroxycyclohexyl benzophenone, benzoin and its derivatives, benzil derivatives, dialkoxyacetophenone, α-hydroxyalkyl benzophenone, benzophenone and its derivatives, vinyl sulfide compounds, diazonium salts, diaryl iodonium salts, triaryl sulfonium salts, alkyl sulfonium salts, and iron aromatic salts.

8. The two-component adhesive for jet printing according to claim 6, Features: The B component includes, in addition to the main resin and the photoinitiator, at least one of an active diluent, a plasticizer, a defoamer, a filler, a dispersant and an inhibitor.

9. A jet printing device using the two-component adhesive for jet printing according to any one of claims 1 to 8, characterized in that: include: A frame, a powder spreading system, a negative pressure ink supply printing system, an ultraviolet lamp system, an infrared heating system, a control system, a forming cylinder system and a material cylinder system. The ultraviolet lamp system is arranged in the moving direction of the powder spreading system.

10. A printing control method for a jet printing device as claimed in claim 9, Features: include: The powder spreading roller pushes the powder above the material cylinder to spread a layer of powder on the forming cylinder; The adhesive printing nozzle sprays the adhesive in the set selected area, and the spraying amount and the number of spraying scans can be adjusted according to the actual situation; The UV lamp is turned on and scanned across the molding cylinder area with the set parameters of light energy density, forward speed and number of scans to perform UV cross-linking and curing on the powder layer surface in the area where the binder is sprayed, and then the UV lamp is turned off; The blank parts are taken out and transferred into the oven for overall heat curing at the preset temperature and holding time to finally obtain high-quality blank parts.