Preparation method and application of toughness balanced polylactic acid blend
By introducing multifunctional block copolymers into polylactic acid, combining PHBV-PDLA hard segment and PCL soft segment, the brittleness problem of polylactic acid material is solved, the balance between strength and toughness is achieved, and the biocompatibility of the material is improved and application potential.
Patent Information
- Application Number
- CN202411372834.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-29
- Publication Date
- 2024-12-06
AI Technical Summary
The inherent brittleness of polylactic acid materials leads to low notch impact strength and elongation of break. The existing methods improve toughness by blending with flexible polymers, but with a decrease in strength and stiffness, making it difficult to achieve a balance between strength and toughness.
Using a multifunctional block copolymer, the ring-opening polymerization reaction of poly(3-hydroxybutyrate-co-3-hydroxyvalerate) and dextrolactide and catalyst were carried out, and caprolactone was added to form PHBV-PDLA. The hard segment and PCL soft segment copolymer are extruded and granulated in combination with antioxidants to prepare a strong and balanced polylactic acid blend.
It effectively improves the toughness of polylactic acid, while maintaining its mechanical strength and biodegradability, making it have wide application potential in product structural parts and packaging fields.
Smart Images

Figure CN119081375A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of polymer materials, and in particular to a preparation method of a strong and tough balanced polylactic acid blend and application thereof. Background Art
[0002] With the increasing concern for natural resources and environmental sustainability, biodegradable materials produced from renewable biomass, such as starch- and sugar-based biomass, have attracted great interest in the past two decades.
[0003] Polylactic acid (PLA) is currently the most commercially available and consumed bio-based polymer. It is fully biorenewable and fully biodegradable, and has great potential to replace petroleum-based non-biodegradable plastics (such as polypropylene and polyethylene terephthalate) due to its ideal biocompatibility, high mechanical strength and stiffness, easy processability, low carbon emissions and competitive price. It has been increasingly used in many applications, including (but not limited to) biomedical devices, packaging, textiles, tableware and some consumer products. Despite this, the industrial production and application of PLA still lags far behind traditional thermoplastic polymers, mainly due to its inherent brittleness, which is characterized by extremely low notched impact strength (~5kJ / m 2 ) and elongation at break (<5%).
[0004] Considerable efforts have been made to improve the toughness of PLA by blending it with various flexible polymers, such as polyethylene (PE), poly(ethylene-glycidyl methacrylate) (EGMA), polyurethane (PU), epoxidized soybean oil (ESO), poly(ε-caprolactone) (PCL), and polybutylene adipate / terephthalate (PBAT). Unfortunately, the introduction of these flexible polymers is accompanied by a significant decrease in strength and stiffness. Therefore, it is necessary to propose a process for preparing PLA that can achieve a balance between strength and toughness. Summary of the invention
[0005] In view of the shortcomings of the prior art, the present invention proposes a method for preparing a strong and tough balanced polylactic acid blend and its application. The multifunctional block copolymer in the present invention can effectively retain the biodegradability and mechanical strength of the polylactic acid material while improving the toughness of the polylactic acid.
[0006] The purpose of the present invention can be achieved through the following technical solutions:
[0007] The first aspect of the present invention relates to a method for preparing a strong and balanced polylactic acid blend, comprising the following steps:
[0008] Poly(3-hydroxybutyrate-co-3-hydroxyvalerate) was dissolved in anhydrous chloroform and subjected to transesterification reaction with methanol solution of H2SO4 to obtain PHBV oligomer intermediate;
[0009] The PHBV oligomer intermediate is used as an initiator, and is injected into a reaction bottle together with dextrorotatory lactide and a catalyst to carry out a ring-opening polymerization reaction;
[0010] After the product of the ring-opening polymerization reaction is cooled, caprolactone is added to continue the reaction, and the obtained product is dissolved in anhydrous chloroform, precipitated with methanol, filtered and dried to obtain a multifunctional block copolymer;
[0011] In parts by weight, 80-95 parts of polylactic acid and 5-20 parts of multifunctional block copolymer are dissolved in anhydrous chloroform, and vacuum dried after being fully dissolved;
[0012] The blend and 0.02-0.1 parts by weight of an antioxidant are added into an extruder for extrusion and granulation.
[0013] Optionally, the poly(3-hydroxybutyrate-co-3-hydroxyvalerate) has a number average molecular weight of 100,000 to 500,000 Daltons and a purity of ≥98%.
[0014] Optionally, the catalyst is selected from at least one of zinc oxide, aluminum isopropoxide, calcium methoxide, tri-n-butyltin methoxide, stannous chloride, and stannous octoate.
[0015] Optionally, the ratio of dextrorotatory lactide D-LA to PHBV and the ratio of dextrorotatory lactide D-LA to catalyst are 2-40:1 and 1500-2500:1, respectively, the polymerization time is 1-3 hours, and the polymerization temperature is 130-150°C.
[0016] Optionally, the mass ratio of caprolactone ε-CL to PHBV oligomer / dextral lactide copolymer intermediate is 0.3-0.7:1, and the reaction is polymerized at 120-140° C. for 1-2 hours, then cooled to 60-80° C. and maintained for 2-4 days.
[0017] Optionally, in the preparation process of the PHBV oligomer intermediate, specifically, polylactic acid and the multifunctional block copolymer are first dissolved in anhydrous chloroform at a concentration of 0.05 to 0.1 g / mL, and the stirring time is 10 to 15 hours to ensure sufficient dissolution; the solution is then poured on a glass culture dish, left at room temperature for 1 to 2 days, and then dried in a 60°C vacuum oven for 10 to 15 hours, and then formed into small pieces using a granulator, and then dried in a 60°C vacuum oven for 10 to 15 hours to ensure complete removal of the solvent.
[0018] Optionally, the antioxidant is at least one of antioxidant CA, antioxidant 168, antioxidant DNP, and antioxidant MB.
[0019] Optionally, the extrusion temperature of the micro extruder is 180-220° C., and the screw speed is 10-50 rpm.
[0020] Optionally, the granulated material can also be injection molded to obtain the final product. The furnace temperature of the micro injection molding machine is set to 190-240°C, the mold temperature is 30-70°C, the injection pressure and time are 700-900 bar, 10-15 seconds, and the holding pressure and time are 400-450 bar, 5-15 seconds.
[0021] The second aspect of the present invention relates to a polylactic acid blend prepared by the above preparation method.
[0022] The third aspect of the present invention relates to the use of the above-mentioned polylactic acid blend in the preparation of product structural parts, shells or packaging.
[0023] Beneficial effects of the present invention:
[0024] The copolymer provided by the present invention is composed not only of a PHBV-PDLA hard segment but also of a PCL soft segment. The PHBV-PDLA hard segment acts as a physical crosslinker for the PCL soft segment matrix. Therefore, the copolymer can enhance the toughness of polylactic acid while maintaining the strength and biodegradability of polylactic acid. The blend of the copolymer and polylactic acid has excellent biocompatibility and can be widely used in the fields of preparing product structural parts, housings or packaging. BRIEF DESCRIPTION OF THE DRAWINGS
[0025] The present invention will be further described below in conjunction with the accompanying drawings.
[0026] Figure 1 Schematic diagram of the synthesis of the multifunctional block copolymer in Example 1 of the present application. DETAILED DESCRIPTION
[0027] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0028] In the following examples and comparative examples of the present application, unless otherwise specified, the reagents and equipment used are conventional commercially available products. The parts used in the examples and comparative examples of the present application are all parts by weight unless otherwise specified.
[0029] Example 1
[0030] In this embodiment, Figure 1As shown, a method for synthesizing a multifunctional block copolymer is disclosed, the purpose of which is to blend with polylactic acid to achieve a balance between the strength and toughness of the polylactic acid material. The multifunctional block copolymer is prepared according to Figure 1 The synthetic schematic diagram of the material comprises the following steps:
[0031] 1. 10g PHBV (number average molecular weight 4×10 5 , purity is 99.5%) was dissolved in 150 mL of anhydrous chloroform, refluxed for 30 minutes, then 100 mL of 5% H2SO4 methanol solution was added to the PHBV solution, stirred with magnetic stirring at 100°C for 30 minutes, cooled to room temperature, filtered, and the product was dried in vacuo at 40°C after removing the solvent;
[0032] 2. Take 5 g of the product PHBV intermediate in 1 as an initiator, place it together with 14.2 g of dextrorotatory lactide (D-LA) and 0.007 g of stannous octoate in a 250 mL reaction bottle at an oil bath temperature of 140°C for ring-opening polymerization for 2 hours;
[0033] 3. After the reaction in 2 has been carried out for 2 hours, let it stand and cool, then add 11.4g of caprolactone (ε-CL), raise the temperature to 130°C and maintain it for 1 hour, then lower it to 80°C and react for 4 days. The reaction product is dissolved in anhydrous chloroform, precipitated with methanol, filtered and dried to obtain a multifunctional block copolymer.
[0034] Next, based on the multifunctional block copolymer prepared in Example 1, polylactic acid blends are further prepared to form Examples 2-5.
[0035] Example 2
[0036] In parts by weight, 95 parts of polylactic acid and 5 parts of multifunctional block copolymer were dissolved in anhydrous chloroform at a concentration of 0.05 g / mL, stirred at room temperature for 12 hours to ensure full dissolution, and then the solution was cast on a glass petri dish to evaporate the solvent for 2 days, dried in a vacuum oven at 60°C for 12 hours, and then made into small pieces using a granulator, and then dried in a vacuum oven at 60°C for 12 hours to ensure complete removal of the solvent. The dried sample and 0.05 parts of antioxidant were added to a micro extruder for extrusion granulation. The extrusion temperature of the micro extruder was 190°C and the screw speed was 30 rpm. The above particles were added to a micro injection molding machine to press the polylactic acid blend strips. The furnace temperature of the micro injection molding machine was 205°C, the mold temperature was 60°C, the injection pressure and time were 900 bar, 15 seconds, and the holding pressure and time were 450 bar, 10 seconds.
[0037] Example 3
[0038] In parts by weight, 90 parts of polylactic acid and 10 parts of multifunctional block copolymer were dissolved in anhydrous chloroform at a concentration of 0.05 g / mL, stirred at room temperature for 12 hours to ensure full dissolution, and then the solution was cast on a glass petri dish to evaporate the solvent for 2 days, dried in a vacuum oven at 60°C for 12 hours, and then formed into small pieces using a granulator, and then dried in a vacuum oven at 60°C for 12 hours to ensure complete removal of the solvent. The dried sample and 0.05 parts of antioxidant were added to a micro extruder for extrusion granulation. The extrusion temperature of the micro extruder was 190°C and the screw speed was 30 rpm. The above particles were added to a micro injection molding machine to press the polylactic acid blend strips. The furnace temperature of the micro injection molding machine was 205°C, the mold temperature was 60°C, the injection pressure and time were 900 bar, 15 seconds, and the holding pressure and time were 450 bar, 10 seconds.
[0039] Example 4
[0040] In parts by weight, 85 parts of polylactic acid and 15 parts of multifunctional block copolymer were dissolved in anhydrous chloroform at a concentration of 0.05 g / mL, stirred at room temperature for 12 hours to ensure full dissolution, and then the solution was cast on a glass petri dish to evaporate the solvent for 2 days, dried in a vacuum oven at 60°C for 12 hours, and then formed into small pieces using a granulator, and then dried in a vacuum oven at 60°C for 12 hours to ensure complete removal of the solvent. The dried sample and 0.05 parts of antioxidant were added to a micro extruder for extrusion granulation. The extrusion temperature of the micro extruder was 190°C and the screw speed was 30 rpm. The above particles were added to a micro injection molding machine to press the polylactic acid blend strips. The furnace temperature of the micro injection molding machine was 205°C, the mold temperature was 60°C, the injection pressure and time were 900 bar, 15 seconds, and the holding pressure and time were 450 bar, 10 seconds.
[0041] Example 5
[0042] In parts by weight, 80 parts of polylactic acid and 20 parts of multifunctional block copolymer were dissolved in anhydrous chloroform at a concentration of 0.05 g / mL, stirred at room temperature for 12 hours to ensure full dissolution, and then the solution was cast on a glass petri dish to evaporate the solvent for 2 days, dried in a vacuum oven at 60°C for 12 hours, and then formed into small pieces using a granulator, and then dried in a vacuum oven at 60°C for 12 hours to ensure complete removal of the solvent. The dried sample and 0.05 parts of antioxidant were added to a micro extruder for extrusion granulation. The extrusion temperature of the micro extruder was 190°C and the screw speed was 30 rpm. The above particles were added to a micro injection molding machine to compress the polylactic acid blend strips. The furnace temperature of the micro injection molding machine was 205°C, the mold temperature was 60°C, the injection pressure and time were 900 bar, 15 seconds, and the holding pressure and time were 450 bar, 10 seconds.
[0043] Comparative Example 1
[0044] The pure polylactic acid particles in the embodiment were injection molded into test specimens.
[0045] The polylactic acid specimens in Examples 2-5 and Comparative Example 1 were subjected to mechanical property tests. The tensile strength and elongation at break were obtained by testing with a universal testing machine in accordance with GB / T 1040.2-2022; the cantilever beam notched impact strength was obtained by testing with a single-arm pendulum impact tester in accordance with GB / T 1843-2008.
[0046] The test results of the mechanical properties of polylactic acid in Examples 2-5 and Comparative Example 1 are shown in the following table:
[0047] As can be seen from the above table, the elongation at break and notched impact strength of the strong and tough balanced polylactic acid prepared by the multifunctional block copolymer in Examples 2-5 of the present invention are better than those in Comparative Example 1, and the tensile strength retention rate is higher. When the addition amount of the multifunctional block copolymer is 15%, the tensile strength retention rate is 80.1%, and the elongation at break increases by about 80 times. This is because the PHBV-PDLA hard segment acts as a physical crosslinker for the PCL soft segment matrix, which effectively maintains the strength of the polylactic acid while greatly improving the toughness of the polylactic acid.
[0048] In the description of this specification, the description with reference to the terms "one embodiment", "example", "specific example", etc. means that the specific features, structures, materials or characteristics described in conjunction with the embodiment or example are included in at least one embodiment or example of the present invention. In this specification, the schematic representation of the above terms does not necessarily refer to the same embodiment or example. Moreover, the specific features, structures, materials or characteristics described can be combined in any one or more embodiments or examples in a suitable manner.
[0049] The above shows and describes the basic principles, main features and advantages of the present invention. Those skilled in the art should understand that the present invention is not limited to the above embodiments, and the above embodiments and descriptions are only for explaining the principles of the present invention. Without departing from the spirit and scope of the present invention, the present invention may have various changes and improvements, and these changes and improvements all fall within the scope of the present invention to be protected.
Claims
1. A method for preparing a strong and balanced polylactic acid blend, characterized in that: The following steps are involved: Poly(3-hydroxybutyrate-co-3-hydroxyvalerate) was dissolved in anhydrous chloroform and subjected to transesterification reaction with methanol solution of H2SO4 to obtain PHBV oligomer intermediate; The PHBV oligomer intermediate is used as an initiator, and is injected into a reaction bottle together with dextrorotatory lactide and a catalyst to carry out a ring-opening polymerization reaction; After the product of the ring-opening polymerization reaction is cooled, caprolactone is added to continue the reaction, and the obtained product is dissolved in anhydrous chloroform, precipitated with methanol, filtered and dried to obtain a multifunctional block copolymer; In parts by weight, 80-95 parts of polylactic acid and 5-20 parts of multifunctional block copolymer are dissolved in anhydrous chloroform, and vacuum dried after being fully dissolved; The blend and 0.02-0.1 parts by weight of an antioxidant are added into an extruder for extrusion granulation.
2. The method for preparing a strong and balanced polylactic acid blend according to claim 1, characterized in that: The number average molecular weight of the poly(3-hydroxybutyrate-co-3-hydroxyvalerate) is 100,000 to 500,000 Daltons, and the purity is ≥98%.
3. The method for preparing a strong and balanced polylactic acid blend according to claim 1, characterized in that: The catalyst is selected from at least one of zinc oxide, aluminum isopropoxide, calcium methoxide, tri-n-butyltin methoxide, stannous chloride, and stannous octoate.
4. The method for preparing a strong and balanced polylactic acid blend according to claim 1, characterized in that: The antioxidant is at least one of antioxidant CA, antioxidant 168, antioxidant DNP and antioxidant MB.
5. The method for preparing a strong and balanced polylactic acid blend according to claim 1, characterized in that: The extrusion temperature of the extruder is 180-220° C., and the screw speed is 10-50 rpm.
6. The method for preparing a strong and balanced polylactic acid blend according to claim 1, characterized in that: The mass ratio of the caprolactone to the product of the ring-opening polymerization reaction is 0.3-0.7:
1.
7. The method for preparing a strong and balanced polylactic acid blend according to claim 1, characterized in that: The mass ratio of the dextrorotatory lactide to poly(3-hydroxybutyrate-co-3-hydroxyvalerate) and the mass ratio of the dextrorotatory lactide to the catalyst are 2-40:1 and 1500-2500:1, respectively.
8. The method for preparing a strong and balanced polylactic acid blend according to claim 1, characterized in that: After extrusion and granulation by extruder, it is molded by injection molding.
9. A polylactic acid blend prepared by the preparation method according to any one of claims 1 to 8.
10. Use of the polylactic acid blend according to claim 9 in preparing product structural parts, shells or packaging.