Tunable porphyrin-cadmium complex Michelene nano nonlinear optical material as well as preparation and application thereof

By preparing tunable porphyrin-cadmium complex mikeene nano-nonlinear optical material, changing the material configuration and coupling degree, the problem of inconsistent performance of two-dimensional nonlinear optical materials is solved, and the selective response to different pulsed lasers is achieved and material stability enhances its application potential in the fields of optical screens and optical switches.

CN119081449AActive Publication Date: 2024-12-06TONGJI UNIV
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411105971.2
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-13
Publication Date
2024-12-06
Estimated Expiration
2044-08-13

AI Technical Summary

Technical Problem

The commercialization of two-dimensional nonlinear optical materials is affected by inconsistent performance and the influence of material structure on nonlinear optical properties. The lack of repeatable synthesis methods and the establishment of structure-performance relationships makes it difficult to improve its nonlinear optical properties.

Method used

By preparing tunable porphyrin-cadmium complex mikeene nano-nonlinear optical material, the bridge group is used to change the material configuration and coupling degree, and improve its nonlinear optical properties, making it selective for lasers of different pulse sizes. . The specific method includes configuring a mixed solution of Mikeene Ti3C2Tx solution and a porphyrin-cadmium complex, performing a stirring reaction, controlling the reaction conditions such as temperature and time, and obtaining conjugated and non-conjugated porphyrin-cadmium complex, respectively. in femtosecond and nanosecond lasers.

Benefits of technology

The selective response of the material to different pulsed lasers is achieved, providing application potential in the field of optical screens and optical switches, and improving the air and light stability of the material, demonstrating a strong correlation between the material structure and nonlinear optical properties.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081449A_ABST
    Figure CN119081449A_ABST
Patent Text Reader

Abstract

The invention relates to a tunable porphyrin-cadmium complex Michelene nano nonlinear optical material as well as preparation and application thereof, two porphyrin-cadmium complexes are designed by utilizing the rotatability of a single bond in an organic matter, and the porphyrin-cadmium complexes are bonded to the surface of two-dimensional few-layer Michelene through substitution reaction bonds. One of the porphyrin-cadmium complexes rotates due to different bridging groups and different steric hindrance, and the conjugation degree of organic components is induced to be greatly changed, so that the two materials respectively respond to lasers with different pulse scales (nanosecond and femtosecond). Compared with the prior art, the material configuration is changed through a bridging group, so that the material coupling degree, the excited state service life and the nonlinear optical performance of the material are changed, and the material has selectivity for lasers with different pulse scales and has good application potential for screening of complex lasers and switching type scenes.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of organic-inorganic hybrid nanomaterials and third-order nonlinear optical materials, and relates to a tunable porphyrin-cadmium complex michaelene nanometer nonlinear optical material and the preparation and application thereof. Background Art

[0002] Nonlinear optics is the basis of many applications, such as harmonic generation, all-optical data processing, information technology, optical sensors, four-wave mixing, etc. With the increasing number of applications of lasers in civil, industrial and academic fields, the research of nonlinear optical (NLO) materials has become the key to the continued development of optoelectronics. Nonlinear optical absorption refers to the phenomenon that the absorption coefficient of a material is different under low and high irradiance light. High-performance nonlinear optical absorption materials are required for pulsed laser generation (mode locking or Q-switching), optical limiting, multiphoton pumped lasers, sub-bandgap photodetection, etc. Among potential nonlinear optical materials, two-dimensional (2D) materials have a particular advantage because of certain advantages such as strong exciton effect, ultrafast carrier dynamics and efficient charge delocalization. Significant progress has been made in the nonlinear optical absorption properties of various 2D materials such as graphene, graphyne, black phosphorus, metal chalcogenides and 2D mixed Ruddlesden-Popper type halide perovskites (RPPs). MXene is a recently developed 2D material with the chemical formula M n+1 X n T x (n = 1-3), where M is a transition metal (such as Ti, Nb, Mo), X is carbon and / or nitrogen, and T is a surface terminal group (such as -O, -OH, -F). The interesting feature of MXene is their excellent electrical conductivity, and they have been used as transparent conductors, electrocatalysts, sensors, electromagnetic interference shielding, energy storage, photothermal conversion, etc. Its nonlinear optical (NLO) properties were first reported by Jhon et al. in 2017, and the nonlinear optical (NLO) properties and applications of MXenes have received increasing attention.

[0003] However, the commercialization of two-dimensional nonlinear optical materials is hampered by inconsistent performance. Their nonlinear optical properties are also closely related to the synthesis method and material structure. Similar structures of the same material may have different or even opposite performance results. In addition, there have been many studies on the effect of the degree of conjugation of the material on the NLO performance. However, in addition to extending the material system, the configuration of the material may also have a significant impact on the degree of conjugation of the material and the final nonlinear optical performance. The distribution of its band structure is very susceptible to the degree of conjugation. Improving nonlinear optical performance requires the development of reproducible synthesis methods and the establishment of structure-performance relationships, but to date, few related studies have been published. Summary of the invention

[0004] The purpose of the present invention is to provide a tunable porphyrin-cadmium complex mikhene nano nonlinear optical material and its preparation and application, and to change the material configuration through a bridging group, thereby changing the material coupling degree, excited state lifetime and its nonlinear optical properties. This strategy makes this type of material selective for lasers of different pulse scales and has good application potential for complex laser screening and switching scenarios.

[0005] The purpose of the present invention can be achieved by the following technical solutions:

[0006] In one aspect, the present invention provides a method for preparing a tunable porphyrin-cadmium complex michaelene nanometer nonlinear optical material, comprising the following steps:

[0007] (1) Configuration of Michaelene Ti3C2T x Solution;

[0008] (2) Dissolve the porphyrin-cadmium complex in a dichloromethane / ethanol mixed solution and transfer it to the mikropicene Ti3C2T x The solution is mixed thoroughly and stirred for reaction, and separated to obtain the target product;

[0009] The porphyrin-cadmium complex is a conjugated porphyrin-cadmium complex 1 and / or a non-conjugated porphyrin-cadmium complex 2;

[0010] The chemical structural formula of the conjugated porphyrin-cadmium complex 1 is:

[0011]

[0012] The chemical structural formula of the non-conjugated porphyrin-cadmium complex 2 is:

[0013]

[0014] Furthermore, the Michaelene Ti3C2T x The mass ratio of porphyrin-cadmium complex is 4:(5-7), preferably 4:6.

[0015] Furthermore, the stirring reaction is carried out under a nitrogen atmosphere, the stirring reaction temperature is 50-70° C., preferably 60° C., and the time is 8-16 h, preferably 12 h.

[0016] Furthermore, before the stirring reaction, K2CO3 was added to the reaction system, which reacted with the mikrophene Ti3C2T x The mass ratio is (2.5-3.5):4, preferably 3:4.

[0017] Furthermore, in the dichloromethane / ethanol mixed solution, the volume ratio of dichloromethane to ethanol is 1:0.8-1.2.

[0018] Furthermore, the porphyrin-cadmium complex is prepared by the following process:

[0019] 5-(4-benzoyl)-10,15,20-triphenylporphyrin or 5-formyl-10,15,20-triphenylporphyrin is prepared by a propionic acid method;

[0020] Under alkaline conditions, 5-(4-benzoyl)-10,15,20-triphenylporphyrin and / or 5-formyl-10,15,20-triphenylporphyrin are used as porphyrin raw materials and reacted with 2-acetylpyridine by Michael addition reaction to obtain tripyridine-substituted porphyrin;

[0021] The tripyridine-substituted porphyrin reacts with cadmium halide to obtain a porphyrin-cadmium complex;

[0022] The chemical structural formula of the tripyridine-substituted porphyrin is:

[0023] (solid hexagons are benzene rings), the corresponding synthesized porphyrin-cadmium complex is conjugated porphyrin-cadmium complex 1; or the chemical structural formula of the tripyridine-substituted porphyrin is The corresponding synthesized porphyrin-cadmium complex is the non-conjugated porphyrin-cadmium complex 2.

[0024] Furthermore, the synthesis of the tripyridine-substituted porphyrin is carried out in steps, firstly dissolving the porphyrin raw material in dichloromethane, adding triethylamine, and performing a reflux reaction once;

[0025] Then, 2-acetylpyridine and triethylamine are added to the reaction system, and reflux is continued for a second time;

[0026] Finally, an excess amount of ammonium acetate ethanol solution was added, and the mixture was refluxed for three times to obtain a brown solution, which was then cooled to room temperature and recrystallized using ethanol to obtain a tripyridine-substituted porphyrin.

[0027] More preferably, the molar ratio of the porphyrin raw material to 2-acetylpyridine is 1:1;

[0028] During the first reflux reaction, the ratio of the added amount of porphyrin raw material, dichloromethane, and triethylamine was 2.5mmol:100mL:10mL;

[0029] During the secondary reflux reaction, the volume ratio of the added triethylamine to dichloromethane was 40:100;

[0030] The time for the first reflux reaction is 6-10 hours, the time for the second reflux reaction is 6-10 hours, and the time for the third reflux reaction is 4-6 hours.

[0031] In a second aspect, the present invention provides a tunable porphyrin-cadmium complex michalene nano nonlinear optical material, which is prepared by any of the above-described preparation methods. Porphyrin-cadmium complex 1 has a benzene ring as a bridge, so that the pyridine complex and porphyrin are conjugated with a high degree of conjugation, and porphyrin-cadmium complex 2 has a large steric hindrance, so that the pyridine complex and porphyrin are perpendicular to each other, and the degree of conjugation is low. The final modified michalene nanosheet has good laser pulse selectivity.

[0032] In a third aspect, the present invention provides an application of a tunable porphyrin-cadmium complex michaelene nanometer nonlinear optical material in a laser pulse selection or switching type laser device. Specifically, the conjugated porphyrin-cadmium complex michaelene nanosheet has an ultrafast response to femtosecond laser, while the non-conjugated porphyrin-cadmium complex michaelene nanosheet only responds to nanosecond laser.

[0033] Furthermore, the laser conditions of the conjugated porphyrin-cadmium complex michelene nanosheets response are 35fs, 5155nm, and 1000Hz.

[0034] Furthermore, the laser conditions of the non-conjugated porphyrin-cadmium complex michelene nanosheets response are 15ns, 532nm and 10 Hz.

[0035] Compared with the prior art, the present invention has the following advantages:

[0036] 1. The porphyrin-cadmium complex michaelene nanometer nonlinear optical material prepared in the present invention has good air and light stability after part of the end groups are replaced.

[0037] 2. The porphyrin-cadmium complex michaelene nano-nonlinear optical material in the present invention has pulse-dependent third-order nonlinear optical properties. The conjugated porphyrin-cadmium complex michaelene nanosheets have an ultrafast response to femtosecond lasers, while the non-conjugated porphyrin-cadmium complex michaelene nanosheets only respond to nanosecond lasers, which proves the strong correlation between material structure and nonlinear optical properties.

[0038] 3. The porphyrin-cadmium complex mikhene nanometer nonlinear optical material prepared in the present invention has good selectivity for pulsed lasers of different scales, can cope with the screening requirements of complex lasers, and has good application potential in the fields of optical screening and optical switching. BRIEF DESCRIPTION OF THE DRAWINGS

[0039] Figure 1 It is a schematic diagram of the specific synthesis process of the conjugated porphyrin-cadmium complex 1 and the non-conjugated porphyrin-cadmium complex 2;

[0040] Figure 2 The figure shows the morphology and element distribution of the porphyrin-cadmium complex michaelene nanometer nonlinear optical material prepared by the present invention;

[0041] Figure 3 This is a film photograph of the porphyrin-cadmium complex michaelene nano nonlinear optical material prepared by the present invention;

[0042] Figure 4 It is an atomic force microscope image and thickness file of the porphyrin-cadmium complex michaelene nano nonlinear optical material prepared by the present invention;

[0043] Figure 5 It is the Z-scan result of the non-conjugated porphyrin-cadmium complex michaelene nano nonlinear optical material prepared by the present invention under nanosecond laser irradiation;

[0044] Figure 6 It is the Z-scan result of the conjugated porphyrin-cadmium complex michaelene nanometer nonlinear optical material prepared by the present invention under femtosecond laser irradiation;

[0045] Figure 7 Schematic diagram of the process of preparing porphyrin-cadmium complex michaelene nano nonlinear optical materials;

[0046] Figure 8 This is the detection diagram of the product prepared in Comparative Example 1. DETAILED DESCRIPTION

[0047] The present invention is described in detail below in conjunction with the accompanying drawings and specific embodiments. This embodiment is implemented based on the technical solution of the present invention, and provides a detailed implementation method and specific operation process, but the protection scope of the present invention is not limited to the following embodiments.

[0048] In the following examples, unless otherwise specified, raw materials or processing techniques are conventional commercial products or conventional processing techniques in the art.

[0049] Embodiment 1:

[0050] The preparation of the conjugated porphyrin-cadmium complex 1 specifically comprises the following steps:

[0051] 5-(4-Benzoyl)-10,15,20-triphenylporphyrin was prepared from references [1] Obtained by synthesis.

[0052] The specific structural chemical formula is as follows:

[0053]

[0054] 2-Acetylpyridine (0.3g, 2.5mmol) and 5-(4-benzoyl)-10,15,20-triphenylporphyrin (1.6g, 2.5mmol) were dissolved in 100mL of dichloromethane, and 10mL of triethylamine was added thereto. The reaction temperature was 40°C and the reaction was refluxed for 8 hours. After the reaction was completed, another molar equivalent of 2-acetylpyridine (0.3g, 2.5mmol) and 40mL of triethylamine were added to the reaction system, and the reaction was monitored in real time by thin layer chromatography. After continuing to reflux at 40°C for 8 hours, acetic acid was added to the reaction system to terminate the reaction and obtain a brown viscous mixture. After the system was detected to be neutral and slightly acidic by pH, an excess of ammonium acetate ethanol solution (1.8g, 25.0mL) was added and refluxed at 70°C for 5 hours to obtain a brown solution. Cool to room temperature and recrystallize from ethanol to obtain tripyridine porphyrin as purple-brown crystals (0.6 g, 40.0%)

[0055] 1 H NMR (CDCl3, 600MHz, TMS, δ / ppm): -2.78(2H,s,-NH),7.31(4H,d,H-Ph),7.67-7.78(8H,m,Hβ-pyrrole),8.05-8.11(8H,m,H Ph),8.22(2H,d,H Ph),8.31(4H,m,H Ph),8.45(1H,m,H Ph),8.51(4H,m,H Py),8.78(2H,d,H Py).

[0056] MS (MALDI-TOF): C 59 H 39 N7 m / z Required: 846.01 Calculated, found: 845.29 [M + ].

[0057] CdBr2 (108.4 mg, 0.4 mmol) was ultrasonically dissolved in 15 mL of ethanol solution, and tripyridine porphyrin (0.3 g, 0.33 mmol) was dissolved in 20 mL of dichloromethane. After ultrasonic dispersion, the supernatants of the two solutions were retained by centrifugation. The cadmium halide solution was slowly added to the upper layer of the porphyrin solution. After standing for 3 days, porphyrin-cadmium complex 1 was obtained.

[0058] MS (MALDI-TOF): C 59 H 39 Br2CdN7 m / z theoretical value: 1117.01 calculated value: 1115.94 [M + ].

[0059] Embodiment 2:

[0060] Preparation of non-conjugated porphyrin-cadmium complex 2:

[0061] 5-Formyl-10,15,20-triphenylporphyrin was prepared from references [2] The preparation method of the non-conjugated porphyrin-cadmium complex 2 is similar to that of the conjugated porphyrin-cadmium complex 1. It is only necessary to replace the reactant 5-(4-benzoyl)-10,15,20-triphenylporphyrin with an equivalent amount of 5-formyl-10,15,20-triphenylporphyrin. The specific steps are as follows:

[0062] 2-Acetylpyridine (0.3g, 2.5mmol) and 5-formyl-10,15,20-triphenylporphyrin (1.4g, 2.5mmol) were dissolved in 100mL of dichloromethane, and 10mL of triethylamine was added thereto, and the reaction was refluxed for 8 hours. After the reaction was completed, another molar equivalent of 2-acetylpyridine (0.3g, 2.5mmol) and 40mL of triethylamine were added to the reaction system, and the reaction was monitored in real time by thin layer chromatography. After continuing to reflux for 8 hours, acetic acid was added to the reaction system to terminate the reaction, and a brown-yellow viscous mixture was obtained. After the system was detected to be neutral and slightly acidic by pH, an excess of ammonium acetate ethanol solution (1.8g, 25.0mL) was continued to be added, and refluxed for 5 hours to obtain a brown solution. After cooling to room temperature, the tripyridine porphyrin without a benzene ring as a bridge was obtained by recrystallization from ethanol, which was brown crystals (0.5g, 35.0%).

[0063] 1 H NMR (CDCl3, 600MHz, TMS, δ / ppm): -2.64(2H,s,-NH),7.71-7.87(8H,m,Hβ-pyrrole),8.24-8.31(8H,m,H Ph),8.45(2H,d,H Ph),8.66(4H,m,H Ph),8.81(1H,m,H Ph),8.91(4H,m,H Py),9.04(2H,d,H Py).

[0064] MS (MALDI-TOF): C 53 H 35 N7 m / z Required: 769.30 Calculated, Found: 768.67 [M + ].

[0065] CdBr2 (108.4 mg, 0.4 mmol) was ultrasonically dissolved in 15 mL of ethanol solution, and the above-mentioned tripyridine porphyrin (0.2 g, 0.33 mmol) was dissolved in 20 mL of dichloromethane. After ultrasonic dispersion, the supernatants of the two solutions were retained by centrifugation. The cadmium halide solution was slowly added to the upper layer of the porphyrin solution. After standing for 3 days, porphyrin-cadmium complex 2 was obtained.

[0066] MS (MALDI-TOF): C 53 H 35 Br2CdN7 m / z theoretical value: 1047.07 calculated value: 1046.00 [M + ].

[0067] Embodiment 3:

[0068] The porphyrin-cadmium complex michaelene nanometer nonlinear optical material specifically comprises the following steps:

[0069] Ti3C2T x According to the literature [3] The etched michelene was dispersed in distilled water in a colloidal form and further freeze-dried to obtain a fluffy solid of about 120 mg.

[0070] Take the above-mentioned Michaelene solid (Ti3C2T x , 4.0 mg) was transferred to a round-bottom flask, anhydrous ethanol (5.0 mL) was added and ultrasonically dispersed to obtain a suspension. The porphyrin cadmium complex obtained in Example 1 or 2 (6.0 mg) was dispersed in 5 mL of anhydrous dichloromethane, and the resulting solution was transferred to the Ti3C2T x To the ethanol suspension, K2CO3 (3 mg) was continuously added. After stirring and refluxed at 60°C for 12 hours under nitrogen protection, the mixture was separated by high-speed centrifugation at 8000 rpm, and the substrate was washed with dichloromethane for multiple times. Part of the sample was placed in a vacuum drying oven to dry, and part of the sample was dispersed in an ethanol solution for testing.

[0071] Comparative Example 1:

[0072] Compared with Examples 1 and 2, tripyridine porphyrin and michelene are directly stirred to verify whether uncomplexed metal ions can cause configurational transformation.

[0073] After testing, tripyridine porphyrin and michelene had no reaction. After sufficient ultrasonic cleaning, it was found that tripyridine porphyrin could not form a stable hybrid material with michelene (see Figure 8 , after sufficient elution, only the absorption of michelene is found, and the tripyridine porphyrin structure in the eluted product remains intact.

[0074] Comparative Example 2:

[0075] Compared with Example 1 or 2, a single solvent is used in the reaction process of tripyridine porphyrin and cadmium halide, which verifies the importance of mixed solvent for complexation reaction.

[0076] It can be seen that tripyridine porphyrin is soluble in organic solvents, and cadmium halide is an inorganic salt. Using a single solvent for the reaction prevents the two from fully reacting. Mass spectrometry verification shows that most of the product is still tripyridine porphyrin, with only a very small amount of complex porphyrin.

[0077] MS (MALDI-TOF): m / z theoretical value: calculated value, 1047.07, found 768.67, a small amount of 1046.00 [M + ].

[0078] Figure 1 Schematic diagram of the specific synthesis process of conjugated porphyrin-cadmium complex 1 and non-conjugated porphyrin-cadmium complex 2, which are obtained by step-by-step Michael addition reaction.

[0079] Figure 2 It is the morphology and element distribution of the conjugated porphyrin-cadmium complex michalene nano nonlinear optical material prepared in Example 3, wherein the presence of N and Cd elements proves that the tripyridine porphyrin in the michalene nanosheets is successfully complexed with the cadmium halide.

[0080] Figure 3 This is a photo of a thin film of the conjugated porphyrin-cadmium complex michaelene nanometer nonlinear optical material prepared in Example 3, proving that this type of material has good dispersibility and high linear optical transmittance;

[0081] Figure 4 The atomic force microscope morphology and thickness file of the conjugated porphyrin-cadmium complex michaelene nano nonlinear optical material prepared in Example 3 dispersed in ethanol, the thickness of which is about 5 nm, proving that the michaelene modified with the porphyrin cadmium complex has fewer layers than the michaelene after etching, and is not easy to agglomerate due to van der Waals forces;

[0082] Figure 5 The two materials prepared in Example 3 were subjected to Z-scan tests under the laser conditions of 35fs, 515nm, 1000Hz and 15ns, 532nm 10 Hz, respectively. The non-conjugated porphyrin-cadmium complex michaelene nano-nonlinear optical material responded under nanosecond laser irradiation, and its minimum modulation depth was 59%, while the conjugated porphyrin-cadmium complex michaelene nano-nonlinear optical material had no absorption under nanosecond laser irradiation.

[0083] Figure 6 The two materials prepared in Example 3 were subjected to Z-scan tests under laser conditions of 35fs, 515nm, 1000Hz and 15ns, 532nm 10 Hz, respectively. The conjugated porphyrin-cadmium complex michaelene nanometer nonlinear optical material responded under femtosecond laser irradiation, and its minimum modulation depth was 23%, while the conjugated porphyrin-cadmium complex michaelene nanometer nonlinear optical material had no absorption under femtosecond laser irradiation.

[0084] At the same time, the two types of porphyrin-cadmium complex michaelene nano-nonlinear optical materials prepared in Example 3 were tested, and it was found that the laser conditions for the response of the conjugated porphyrin-cadmium complex michaelene nanosheets were 35fs, 5155nm, 1000Hz; the laser conditions for the response of the non-conjugated porphyrin-cadmium complex michaelene nanosheets were 15ns, 532nm10 Hz.

[0085] Based on the above, we can know that the porphyrin-cadmium complex michalene nano nonlinear optical material changes the steric hindrance between the tripyridine cadmium complex unit and the porphyrin unit through the simplest bridging group benzene ring, so that the two porphyrins and cadmium complexes are in a conjugated relationship and perpendicular to each other, and the configuration changes significantly. The change in configuration changes the degree of conjugation of the porphyrin cadmium complex, thereby affecting its energy level arrangement, linear absorption and excited state lifetime, and ultimately changing its nonlinear optical properties.

[0086] At the same time, its different conjugated structure enables this type of material to produce nonlinear responses under nanosecond and femtosecond pulse lasers, respectively, making it one of the important candidate materials for screening different pulse lasers and optical switches.

[0087] The above description of the embodiments is to facilitate the understanding and use of the invention by those skilled in the art. It is obvious that those skilled in the art can easily make various modifications to these embodiments and apply the general principles described herein to other embodiments without creative work. Therefore, the present invention is not limited to the above embodiments, and improvements and modifications made by those skilled in the art based on the disclosure of the present invention without departing from the scope of the present invention should be within the scope of protection of the present invention.

Claims

1. A method for preparing a tunable porphyrin-cadmium complex michaelene nanometer nonlinear optical material, characterized in that: The following steps are involved: (1) Configuration of Michaelene Ti3C2T x Solution; (2) Dissolve the porphyrin-cadmium complex in a dichloromethane / ethanol mixed solution and transfer it to the mikropicene Ti3C2T x The solution is mixed thoroughly and stirred for reaction, and separated to obtain the target product; The porphyrin-cadmium complex is a conjugated porphyrin-cadmium complex 1 and / or a non-conjugated porphyrin-cadmium complex 2; The chemical structural formula of the conjugated porphyrin-cadmium complex 1 is: The chemical structural formula of the non-conjugated porphyrin-cadmium complex 2 is:

2. The method for preparing a tunable porphyrin-cadmium complex michaelene nanometer nonlinear optical material according to claim 1, characterized in that: The Mikeene Ti3C2T x , the mass ratio of porphyrin-cadmium complex is 4:(5~7).

3. The method for preparing a tunable porphyrin-cadmium complex michaelene nanometer nonlinear optical material according to claim 1, characterized in that: The stirring reaction is carried out under a nitrogen atmosphere at a temperature of 50-70° C. for 8-16 h.

4. The method for preparing a tunable porphyrin-cadmium complex michaelene nanometer nonlinear optical material according to claim 1, characterized in that: Before stirring the reaction, K2CO3 was added to the reaction system, which reacted with the mikrophenone Ti3C2T x The mass ratio is (2.5~3.5):

4.

5. The method for preparing a tunable porphyrin-cadmium complex michaelene nanometer nonlinear optical material according to claim 1, characterized in that: In the dichloromethane / ethanol mixed solution, the volume ratio of dichloromethane to ethanol is 1:0.8-1.

2.

6. The method for preparing a tunable porphyrin-cadmium complex michaelene nanometer nonlinear optical material according to claim 1, characterized in that: The porphyrin-cadmium complex is prepared by the following process: 5-(4-benzoyl)-10,15,20-triphenylporphyrin or 5-formyl-10,15,20-triphenylporphyrin is prepared by a propionic acid method; Under alkaline conditions, 5-(4-benzoyl)-10,15,20-triphenylporphyrin and / or 5-formyl-10,15,20-triphenylporphyrin are used as porphyrin raw materials and reacted with 2-acetylpyridine by Michael addition reaction to obtain tripyridine-substituted porphyrin; The tripyridine-substituted porphyrin reacts with cadmium halide to obtain a porphyrin-cadmium complex; The chemical structural formula of the tripyridine-substituted porphyrin is: The corresponding synthesized porphyrin-cadmium complex is a conjugated porphyrin-cadmium complex 1; or the chemical structural formula of the tripyridine-substituted porphyrin is The corresponding synthesized porphyrin-cadmium complex is the non-conjugated porphyrin-cadmium complex 2.

7. The method for preparing a tunable porphyrin-cadmium complex michaelene nanometer nonlinear optical material according to claim 6, characterized in that: The synthesis of tripyridine-substituted porphyrin is carried out in steps. First, the porphyrin raw material is dissolved in dichloromethane, triethylamine is added, and a reflux reaction is performed once; Then, 2-acetylpyridine and triethylamine are added to the reaction system, and reflux is continued for a second time; Finally, an excess amount of ammonium acetate ethanol solution was added, and the mixture was refluxed for three times to obtain a brown solution, which was then cooled to room temperature and recrystallized using ethanol to obtain a tripyridine-substituted porphyrin.

8. The method for preparing a tunable porphyrin-cadmium complex michaelene nanometer nonlinear optical material according to claim 7, characterized in that: The molar ratio of porphyrin raw material and 2-acetylpyridine is 1:1; During the first reflux reaction, the ratio of the added amount of porphyrin raw material, dichloromethane, and triethylamine was 2.5mmol:100mL:10mL; During the secondary reflux reaction, the volume ratio of the added triethylamine to dichloromethane was 40:100; The time for the first reflux reaction is 6-10 hours, the time for the second reflux reaction is 6-10 hours, and the time for the third reflux reaction is 4-6 hours.

9. A tunable porphyrin-cadmium complex michaelene nanometer nonlinear optical material, which is prepared by the preparation method according to any one of claims 1 to 8.

10. Use of the tunable porphyrin-cadmium complex michaelene nanometer nonlinear optical material as claimed in claim 9 in laser pulse selection or switching type laser devices.

Citation Information

Patent Citations

  • Cationic porphyrin functionalized Ti3C2Tx nanosheet nonlinear nano hybrid material as well as preparation and application thereof

    CN113773835A

  • Porphyrin covalent functionalized Ti3C2Tx nanosheet nonlinear nano hybrid material as well as preparation and application of porphyrin covalently functionalized Ti3C2Tx nanosheet nonlinear nano hybrid material

    CN113831350A

  • Element having porphyrin polymer fixed on a substrate and method of preparing the same

    US20040202876A1

  • Heteroporphyrin nanotubes and composites

    US7132163B1

  • Lithium ion- or sodium ion-based internal hybrid electrochemical energy storage cell

    WO2019070568A2