Novel heavy-duty anti-corrosion environment-friendly material for multifunctional liquid ceramic

By using polyurethane modified nanoceramic emulsion, modified graphene and nanosilicon sol in anticorrosion coatings, the problem of poor compatibility between fillers and resins is solved, forming a high-hardness corrosion-resistant coating, and improving the comprehensiveness of anticorrosion coatings Performance, higher weather resistance and heat resistance, and environmentally friendly and non-toxic.

CN119081454AInactive Publication Date: 2024-12-06北京优龙前沿新材料技术研究院有限公司
View PDF 6 Cites 0 Cited by

Patent Information

Application Number
CN202410761989.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-06-13
Publication Date
2024-12-06
Estimated Expiration
Not applicable · inactive patent

AI Technical Summary

Technical Problem

The compatibility between fillers and film-forming resin in existing anticorrosion coatings is poor, resulting in a large number of pinholes and gaps easily forming at the interface, reducing the anti-corrosion effect of the material.

Method used

Polyurethane modified nanoceramic emulsion, modified graphene, nanosilica sol, silane coupling agent and aminosilane curing agent are used to form a high-hardness and corrosion-resistant coating through spraying or dipping coating to improve the dispersion of fillers and curing reaction to enhance corrosion resistance.

Benefits of technology

The formation of a high-hardness and corrosion-resistant coating improves the dispersion effect of fillers, improves the comprehensive performance of anticorrosive coatings, has higher weather resistance and heat resistance, low odor, and is non-toxic and environmentally friendly.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention discloses a novel heavy-duty environment-friendly material for multifunctional liquid ceramics, which is prepared from the following components in parts by weight: 45 to 60 parts of polyurethane modified nano ceramic emulsion, 1 to 20 parts of high-temperature-resistant pigment, 1 to 25 parts of filler, 0.1 to 3 parts of fumed silica, 0.1 to 1.5 parts of wetting dispersant, 0.01 to 3 parts of defoaming agent, 0.1 to 2 parts of corrosion inhibitor, 0.1 to 0.5 part of modified graphene, 0.1 to 3 parts of p-toluenesulfonic acid amine neutralizer and 0.1 to 1.5 parts of thickening agent. According to the present invention, the nanometer silica sol is adopted as the main body resin, is matched with the silane coupling agent, and is compounded with the certain catalyst, such that the coating with characteristics of high hardness, corrosion resistance, good gloss and ceramic glaze texture can be formed after baking, and the dispersion effect of the pigment filler in the anti-corrosion coating can be effectively improved;
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of a new multifunctional liquid ceramic heavy-duty anti-corrosion and environmentally friendly material, in particular to a new multifunctional liquid ceramic heavy-duty anti-corrosion and environmentally friendly material. Background Art

[0002] Ceramic coating is a new type of coating material based on organic-inorganic hybrid technology. Since its main structure is a covalently cross-linked inorganic (metal oxide, non-metal oxide, etc.) network, it has many performance advantages that traditional organic coatings cannot match, such as high hardness, friction resistance, flame retardancy, super weather resistance, low surface energy, and chemical solvent resistance. After searching, the Chinese patent authorization number CN112094514B discloses a high-toughness water-based ceramic coating. Although the material is easy to construct, has extremely low VOC emissions during coating, and has excellent flame retardancy, heat resistance, corrosive medium shielding, bending resistance, and impact resistance, it is an excellent choice for high-temperature resistance and high-durability anti-corrosion protective coatings. However, the compatibility between the filler and the film-forming resin in the anti-corrosion coating is poor, and a large number of pinholes and gaps are easily formed between the interface between the two, reducing the anti-corrosion effect of the material. Summary of the invention

[0003] In view of the shortcomings of the prior art, the present invention provides a new environmentally friendly material for multifunctional liquid ceramic heavy-duty corrosion protection, which solves the problem mentioned in the background technology that the compatibility between fillers and film-forming resins in existing anti-corrosion coatings is poor, and a large number of pinholes and gaps are easily formed between the interfaces of the two, thereby reducing the anti-corrosion effect of the material.

[0004] To achieve the above purpose, the present invention is implemented through the following technical scheme: a new material for multifunctional liquid ceramic heavy-duty corrosion protection and environmental protection, whose components include the following: 45-60 parts of polyurethane modified nano-ceramic emulsion, 1-20 parts of high temperature resistant pigment, 1-25 parts of filler, 0.1-3 parts of fumed silica, 0.1-1.5 parts of wetting dispersant, 0.01-3 parts of defoamer, 0.1-2 parts of corrosion inhibitor, 0.1-0.5 parts of modified graphene, 0.1-3 parts of p-toluenesulfonic acid amine neutralizer, 0.1-1.5 parts of thickener, 0.1-0.5 parts of nano-silica sol, and 0.1-2 parts of curing agent.

[0005] Preferably, the nano silica sol is prepared by adding organic silicon into an acetone solvent in a weight ratio of 1:5, then adding 2-5 parts of ammonia water and 1-4 parts of a silane coupling agent, first stirring at a constant speed of 150-200 r / min for 10-20 min, then adding 5-10 parts of activated epoxy resin, reacting at 40-45° C. for 20-30 min, and the reaction speed is 70-100 r / min. The reaction is completed to obtain the nano silica sol.

[0006] Preferably, the polyurethane modified nano ceramic emulsion is prepared by adding polyethylene glycol, polycarbonate diol and neopentyl glycol to a deoxygenated reactor, heating to 100-150° C., and dehydrating under reduced pressure; cooling to below 50° C., adding acetone, and stirring to completely dissolve the materials; diluting hexamethylene diisocyanate and isophorone diisocyanate with acetone, and then slowly dripping them into the reactor; adding di-n-butyltin dilaurate, heating to reflux and stirring to react for 3-4 hours; cooling the system to below 40° C., adding organosilane, stirring evenly, and then adding it to a mixed solution consisting of silica sol, sodium ethylenediamine sulfonate and water; heating to 60-70° C., keeping the temperature for 1-3 hours, and then removing acetone in the system under reduced pressure; cooling and filtering, a polyurethane modified nano ceramic emulsion with a non-volatile content of 35-50% can be obtained.

[0007] Preferably, the filler is one or more of quartz powder, whisker silicon, aluminum oxide, silicon carbide, barium sulfate, and titanium oxide, and the particle size is controlled within 30 μm.

[0008] Preferably, the modified graphene is dispersed in deionized water through graphite oxide, ultrasonically dispersed to obtain a 10 mg / mL dispersion, 20-30 mg of thiourea is added, ultrasonically dispersed, 25-30 mg of cobalt nitrate is added, ultrasonically dispersed, 1-2 mL of formaldehyde is added, 300-350 mg of urea is added, stirred until it is fluffy and resinous, and finally placed in a high-pressure reactor, hydrothermal at 180-200° C. for 8 hours. After the reaction is completed, the reaction product is placed in a freeze drying oven for drying to obtain a precursor I, and then the precursor I is placed in a sulfuric acid solution with a concentration of 1-2 mol / L, stirred and repeatedly pickled at 80° C. until the cobalt atoms on the surface of the precursor I are completely removed, and finally the pickled product is washed with water and dried to obtain the modified graphene.

[0009] Preferably, the thickener is a polyurethane thickener, and the wetting and dispersing agent is KF-7619 segment polymer.

[0010] Preferably, the curing agent component includes 35-75% of aminosilane, 2-5% of surfactant and the balance is water.

[0011] Preferably, the aminosilane is at least one of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, bis(3-trimethoxysilylpropyl)amine, N-cyclohexyl-γ-aminopropylmethyldimethoxysilane, and N-cyclohexyl-γ-aminopropyltrimethoxysilane, and the surfactant is at least one of a cationic surfactant, an anionic surfactant, and a nonionic surfactant.

[0012] Preferably, the silane coupling agent is at least one of A171, KH550, KH580, KH590, KH792, and DL602.

[0013] The finished product is obtained by mixing and stirring the components uniformly and treating the mixture at a temperature of 30-40° C. for 2-5 hours.

[0014] The present invention provides a new material for multifunctional liquid ceramic heavy-duty corrosion protection and environmental protection. It has the following beneficial effects:

[0015] The invention relates to a new environmentally friendly material for multifunctional liquid ceramic heavy-duty corrosion protection, which uses nano-silica sol as the main resin, is matched with a silane coupling agent, and is compounded with a certain catalyst. It reaches the surface of ceramics or metals by spraying or dipping, and can form a coating with high hardness, corrosion resistance, good gloss and ceramic glaze texture after baking. The silane coupling agent is added, which can effectively improve the dispersibility of modified graphene and pigments and fillers in the coating system, which is very beneficial to improving the comprehensive performance of the anti-corrosion coating. Adjacent modified graphene molecules cooperate with each other to form a relatively tight physical barrier, which can not only prevent physical contact between adjacent pigments and fillers to the greatest extent, but also effectively improve the dispersion effect of pigments and fillers in the anti-corrosion coating. At the same time, the silanol in the curing agent in the material is aminosilanol obtained by hydrolysis of aminosilane, which has both inorganic silanol condensation properties and organic ammonia catalytic properties. It has higher weather resistance and heat resistance than traditional amine curing agents, milder curing reaction, lower odor, non-toxic and more environmentally friendly. DETAILED DESCRIPTION

[0017] The following will be combined with the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0018] Embodiment 1:

[0019] A new environmentally friendly material for multifunctional liquid ceramic heavy-duty corrosion protection, comprising the following ingredients: 60 parts of polyurethane modified nano-ceramic emulsion, 20 parts of high temperature resistant pigment, 25 parts of filler, 3 parts of fumed silica, 1.5 parts of wetting dispersant, 3 parts of defoamer, 2 parts of corrosion inhibitor, 0.5 parts of modified graphene, 3 parts of p-toluenesulfonic acid amine neutralizer, 1.5 parts of thickener, 0.5 parts of nano-silica sol, and 2 parts of curing agent.

[0020] Nano silica sol is prepared by adding organic silicon into acetone solvent in a weight ratio of 1:5, then adding 5 parts of ammonia water and 4 parts of silane coupling agent, stirring at a constant speed of 200 r / min for 20 minutes, and then adding 10 parts of activated epoxy resin, reacting at 45°C for 30 minutes, and the reaction speed is 100 r / min. After the reaction is completed, nano silica sol is obtained; polyurethane modified nano ceramic emulsion is prepared by adding polyethylene glycol, polycarbonate diol and neopentyl glycol into a deoxygenated reactor, heating to 150°C, and decompressing and dehydrating; cooling To 40°C, add acetone, stir to completely dissolve the materials; dilute hexamethylene diisocyanate and isophorone diisocyanate with acetone, and then slowly drip into the reactor; add di-n-butyltin dilaurate, heat reflux and stir to react for 4 hours; cool the system to 30°C, add organosilane, stir well, and then add to the mixed solution of silica sol, sodium ethylenediamine sulfonate and water; heat to 70°C, keep warm for 3 hours, and then reduce the pressure to remove acetone in the system; cool and filter to obtain a polyurethane modified with a non-volatile content of 50%. The filler is quartz powder, and the particle size is controlled within 30 μm; the modified graphene is dispersed in deionized water by graphite oxide, and ultrasonic dispersion is uniformly obtained to obtain a 10 mg / mL dispersion, 30 mg of thiourea is added, ultrasonic dispersion is uniformly obtained, and then 30 mg of cobalt nitrate is added, ultrasonic dispersion is uniformly obtained, 2 mL of formaldehyde is added, 350 mg of urea is added, and stirring is performed until the mixture is fluffy and resinous, and finally the mixture is placed in a high-pressure reactor, and hydrothermal reaction is performed at 200°C for 8 hours. After the reaction is completed, the reaction product is placed in a freeze drying oven for drying to obtain a precursor. I, and then the precursor I is placed in a sulfuric acid solution with a concentration of 2 mol / L, and is repeatedly pickled with stirring at 80°C until the cobalt atoms on the surface of the precursor I are completely removed, and finally the pickled product is washed with water and dried to obtain modified graphene; the thickener is a polyurethane thickener, and the wetting and dispersing agent KF-7619 is a segmented polymer; the curing agent component includes 75% of aminosilane, 5% of surfactant, and the balance is water; the aminosilane is 3-aminopropyltrimethoxysilane, and the surfactant is a cationic surfactant; the silane coupling agent is A171.

[0021] The components are mixed and stirred uniformly, and the mixture is mixed at 30° C. for 2 hours to obtain a finished product.

[0022] Embodiment 2:

[0023] A new environmentally friendly material for multifunctional liquid ceramic heavy-duty corrosion protection, comprising the following ingredients: 45 parts of polyurethane modified nano-ceramic emulsion, 1 part of high temperature resistant pigment, 1 part of filler, 0.1 part of fumed silica, 0.1 part of wetting dispersant, 0.01 part of defoamer, 0.1 part of corrosion inhibitor, 0.1 part of modified graphene, 0.1 part of p-toluenesulfonic acid amine neutralizer, 0.1 part of thickener, 0.1 part of nano-silica sol, and 0.1 part of curing agent.

[0024] Nano silica sol is prepared by adding organic silicon into acetone solvent in a weight ratio of 1:5, then adding 2 parts of ammonia water and 1 part of silane coupling agent, stirring at a constant speed of 150r / min for 10min, then adding 5 parts of activated epoxy resin, reacting at 40°C for 20min, and the reaction speed is 70r / min. After the reaction is completed, nano silica sol is obtained; polyurethane modified nano ceramic emulsion is prepared by adding polyethylene glycol, polycarbonate diol and neopentyl glycol into a deoxygenated reactor, heating to 100°C, decompressing and dehydrating; cooling to 20°C, Add acetone and stir to completely dissolve the materials; dilute hexamethylene diisocyanate and isophorone diisocyanate with acetone, and then slowly drip into the reactor; add di-n-butyltin dilaurate, heat and reflux and stir to react for 3 hours; cool the system to 25°C, add organosilane, stir evenly, and then add to the mixed solution of silica sol, sodium ethylenediamine sulfonate and water; heat to 60°C, keep warm for 1 hour, and then remove acetone in the system under reduced pressure; cool and filter to obtain a polyurethane modified nano-ceramic emulsion with a non-volatile content of 35%; The fillers are aluminum oxide, silicon carbide, and barium sulfate, and the particle size is controlled within 30 μm; the modified graphene is dispersed in deionized water by graphite oxide, and ultrasonic dispersion is uniformly performed to obtain a 10 mg / mL dispersion liquid, 20 mg of thiourea is added, and ultrasonic dispersion is uniformly performed, and then 25 mg of cobalt nitrate is added, and ultrasonic dispersion is uniformly performed, 1 mL of formaldehyde is added, and 300 mg of urea is added, and the mixture is stirred until it becomes a fluffy resin, and finally placed in a high-pressure reactor, and hydroheated at 180° C. for 8 hours. After the reaction is completed, the reaction product is placed in a freeze drying oven for drying to obtain a precursor I, and then The precursor I is placed in a sulfuric acid solution with a concentration of 1 mol / L, and is repeatedly pickled with stirring at 80°C until the cobalt atoms on the surface of the precursor I are completely removed. Finally, the pickled product is washed with water and dried to obtain modified graphene; the thickener is a polyurethane thickener, and the wetting and dispersing agent is KF-7619 segmented polymer; the curing agent component includes 35-75% of aminosilane, 2-5% of surfactant, and the balance is water; the aminosilane is 3-aminopropyltriethoxysilane, the surfactant is an anionic surfactant; and the silane coupling agent is KH550.

[0025] The finished product is obtained by mixing and stirring the components uniformly and treating the mixture at 35° C. for 3.5 hours.

[0026] Embodiment 3:

[0027] A new environmentally friendly material for multifunctional liquid ceramic heavy-duty corrosion protection, comprising the following ingredients: 50 parts of polyurethane modified nano-ceramic emulsion, 15 parts of high temperature resistant pigment, 15 parts of filler, 2 parts of fumed silica, 1.2 parts of wetting dispersant, 2 parts of defoamer, 0.5 parts of corrosion inhibitor, 0.3 parts of modified graphene, 2 parts of p-toluenesulfonic acid amine neutralizer, 1.2 parts of thickener, 0.8 parts of nano-silica sol, and 1 part of curing agent.

[0028] Nano silica sol is prepared by adding organic silicon into acetone solvent in a weight ratio of 1:5, then adding 3 parts of ammonia water and 3 parts of silane coupling agent, stirring at a constant speed of 160r / min for 15min, then adding 8 parts of activated epoxy resin, reacting at 42°C for 25min, and the reaction speed is 75r / min. After the reaction is completed, nano silica sol is obtained; polyurethane modified nano ceramic emulsion is prepared by adding polyethylene glycol, polycarbonate diol and neopentyl glycol into a deoxygenated reactor, heating to 120°C, dehydrating under reduced pressure, and cooling to below 50°C , add acetone, stir to completely dissolve the materials; dilute hexamethylene diisocyanate and isophorone diisocyanate with acetone, and then slowly drip into the reactor; add di-n-butyltin dilaurate, heat reflux and stir to react for 2 hours; cool the system to 35°C, add organosilane, stir evenly, and then add to the mixed solution of silica sol, sodium ethylenediamine sulfonate and water; heat to 65°C, keep warm for 2 hours, and then remove acetone in the system under reduced pressure; cool and filter to obtain a polyurethane modified nano-ceramic emulsion with a non-volatile content of 40%. The fillers are barium sulfate and titanium oxide, and the particle size is controlled within 30 μm; the modified graphene is dispersed in deionized water by graphite oxide, and ultrasonic dispersion is uniformly obtained to obtain a 10 mg / mL dispersion liquid, 25 mg of thiourea is added, ultrasonic dispersion is uniformly obtained, and then 27 mg of cobalt nitrate is added, ultrasonic dispersion is uniformly obtained, 1.5 mL of formaldehyde is added, 320 mg of urea is added, and stirring is performed until the precursor I is fluffy and resinous, and finally the precursor I is placed in a high-pressure reactor and hydrothermal heated at 190°C for 8 hours. After the reaction is completed, the reaction product is placed in a freeze drying oven for drying to obtain a precursor I, and then the precursor I is placed in a high-pressure reactor and hydrothermal heated at 190°C for 8 hours. The precursor I is placed in a sulfuric acid solution with a concentration of 1.5 mol / L, and is repeatedly acid-washed at 80°C with stirring until the cobalt atoms on the surface of the precursor I are completely removed. Finally, the acid-washed product is washed with water and dried to obtain modified graphene; the thickener is a polyurethane thickener, and the wetting and dispersing agent is KF-7619 segment polymer; the curing agent component includes 40% aminosilane, 4% surfactant, and the balance is water; the aminosilane is N-cyclohexyl-γ-aminopropyltrimethoxysilane, the surfactant is a cationic surfactant; the silane coupling agent is DL602. The components are mixed and stirred evenly, and the finished product is obtained after mixing and treating at a temperature of 40°C for 5 hours.

[0029] Comparative Example 1:

[0030] A new material for multifunctional liquid ceramic heavy-duty anti-corrosion and environmental protection, comprising the following ingredients: 50 parts of polyurethane modified nano-ceramic emulsion, 10 parts of high temperature resistant pigment, 10 parts of filler, 2 parts of fumed silica, 1 part of wetting dispersant, 1.5 parts of defoamer, 1 part of corrosion inhibitor, 1 part of thickener, 0.2 parts of water-based resin, and 1 part of amine curing agent;

[0031] Table 1 Comparison of physical and chemical tests of materials

[0032]

[0033]

[0034] CK is a common new anti-corrosion material available on the market. Table 1 shows that adding silane coupling agent effectively improves the dispersibility of modified graphene and pigments and fillers in the coating system, which is very beneficial to improving the comprehensive performance of anti-corrosion coatings. It can not only prevent physical contact between adjacent pigments and fillers, but also effectively improve the dispersion effect of pigments and fillers in anti-corrosion coatings. Silanol is aminosilanol obtained by hydrolysis of aminosilane. It has both the polycondensation characteristics of inorganic silanol and the catalytic characteristics of organic ammonia. It has higher weather resistance and heat resistance than traditional amine curing agents, milder curing reaction, low odor, non-toxic and more environmentally friendly. The product of the present invention is superior to commercial products in hardness, wear resistance, alkali acid resistance, and salt spray resistance.

[0035] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the appended claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention.

[0036] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A new material for multifunctional liquid ceramic heavy-duty anti-corrosion and environmental protection, Features: The ingredients include: 45-60 parts of polyurethane modified nano-ceramic emulsion, 1-20 parts of high temperature resistant pigment, 1-25 parts of filler, 0.1-3 parts of fumed silica, 0.1-1.5 parts of wetting dispersant, 0.01-3 parts of defoamer, 0.1-2 parts of corrosion inhibitor, 0.1-0.5 parts of modified graphene, 0.1-3 parts of p-toluenesulfonic acid amine neutralizer, 0.1-1.5 parts of thickener, 0.1-0.5 parts of nano-silica sol and 0.1-2 parts of curing agent.

2. According to claim 1, a new material for multifunctional liquid ceramic heavy-duty anti-corrosion and environmental protection, Features: The nano silica sol is prepared by adding organic silicon into an acetone solvent at a weight ratio of 1:5, then adding 2-5 parts of ammonia water and 1-4 parts of a silane coupling agent, first stirring at a constant speed of 150-200 r / min for 10-20 minutes, then adding 5-10 parts of activated epoxy resin, reacting at 40-45° C. for 20-30 minutes at a reaction speed of 70-100 r / min, and then completing the reaction to obtain the nano silica sol.

3. According to claim 1, a new material for multifunctional liquid ceramic heavy-duty anti-corrosion and environmental protection, Features: The polyurethane modified nano ceramic emulsion is prepared by adding polyethylene glycol, polycarbonate diol and neopentyl glycol into a deoxygenated reactor, heating to 100-150° C., and dehydrating under reduced pressure; cooling to below 50° C., adding acetone, and stirring to completely dissolve the materials; diluting hexamethylene diisocyanate and isophorone diisocyanate with acetone, and then slowly dripping them into the reactor; adding di-n-butyltin dilaurate, heating to reflux and stirring to react for 3-4 hours; cooling the system to below 40° C., adding organic silane, stirring evenly, and then adding it to a mixed solution consisting of silica sol, sodium ethylenediamine sulfonate and water; heating to 60-70° C., keeping the temperature for 1-3 hours, and then removing acetone in the system under reduced pressure; cooling, filtering, and obtaining the polyurethane modified nano ceramic emulsion with a non-volatile content of 35-50%.

4. According to claim 1, a new material for multifunctional liquid ceramic heavy-duty anti-corrosion and environmental protection, Features: The filler is one or more of quartz powder, whisker silicon, aluminum oxide, silicon carbide, barium sulfate, and titanium oxide, and the particle size is controlled within 30 μm.

5. According to claim 1, a new material for multifunctional liquid ceramic heavy-duty anti-corrosion and environmental protection, Features: The modified graphene is dispersed in deionized water by graphite oxide, and ultrasonically dispersed to obtain a 10 mg / mL dispersion, 20-30 mg of thiourea is added, and ultrasonically dispersed to obtain a 10 mg / mL dispersion, 25-30 mg of cobalt nitrate is added, and ultrasonically dispersed to obtain a 10 mg / mL dispersion, 1-2 mL of formaldehyde is added, 300-350 mg of urea is added, and the mixture is stirred until it becomes a fluffy resin, and finally placed in a high-pressure reactor, and hydrothermal treatment is performed at 180-200° C. for 8 hours. After the reaction is completed, the reaction product is placed in a freeze drying oven for drying to obtain a precursor I, and then the precursor I is placed in a sulfuric acid solution with a concentration of 1-2 mol / L, and acid-washed repeatedly at 80° C. with stirring until the cobalt atoms on the surface of the precursor I are completely removed, and finally the acid-washed product is washed with water and dried to obtain the modified graphene.

6. According to claim 1, a new material for multifunctional liquid ceramic heavy-duty anti-corrosion and environmental protection, Features: The thickener is a polyurethane thickener, and the wetting and dispersing agent KF-7619 is a segmented polymer.

7. According to claim 1, a new material for multifunctional liquid ceramic heavy-duty anti-corrosion and environmental protection, Features: The curing agent component comprises 35-75% of aminosilane, 2-5% of surfactant and the balance is water.

8. According to claim 7, a multifunctional liquid ceramic heavy-duty anti-corrosion and environmentally friendly new material, Features: The aminosilane is at least one of 3-aminopropyltrimethoxysilane, 3-aminopropyltriethoxysilane, bis(3-trimethoxysilylpropyl)amine, N-cyclohexyl-γ-aminopropylmethyldimethoxysilane, and N-cyclohexyl-γ-aminopropyltrimethoxysilane; the surfactant is at least one of a cationic surfactant, an anionic surfactant, and a nonionic surfactant; and the silane coupling agent is at least one of A171, KH550, KH580, KH590, KH792, and DL602.

9. A method for preparing a multifunctional liquid ceramic heavy-duty anti-corrosion and environmentally friendly new material according to any one of claims 1 to 8, Features: The finished product is obtained by mixing and stirring the components uniformly and treating the mixture at a temperature of 30-40° C. for 2-5 hours.

Citation Information

Patent Citations

  • A water-based ceramic coating and its preparation method

    CN112094514B

  • Aqueous inorganic nano ceramic paint curing agent and preparation method thereof

    CN109294318A

  • Water-based ceramic coating and preparation method thereof

    CN112094514A

  • Production process of water-based nano ceramic coating

    CN112409829A

  • Nanoceramic anticorrosive water-based paint

    CN113045976A