Powder coating free of puttying and painting as well as preparation method and use method of powder coating

A powdered coating with high-alumina white cement and latex powder enhances adhesion and hardness, allowing direct application without putty or paint, addressing the inefficiencies of existing non-toxic coatings.

CN119081457APending Publication Date: 2024-12-06FU JIAN HAI YAO LV LAN XIN CAI LIAO YOU XIAN GONG SI
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411148000.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-21
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing non-toxic powder coatings require multiple layers of putty and paint application, which is time-consuming and labor-intensive, and lack sufficient adhesion and hardness.

Method used

A powdered coating composition comprising high-alumina white cement, cellulose, bentonite, early strength agent, latex powder, and colored sand, which is mixed without the need for puttying or painting, using a zero-gravity mixer to achieve enhanced adhesion and hardness.

Benefits of technology

The coating provides direct application without putty or paint, ensuring strong adhesion, durability, and color, while being free from formaldehyde, toluene, and VOCs, with improved efficiency and reduced labor.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081457A_ABST
    Figure CN119081457A_ABST
Patent Text Reader

Abstract

The invention discloses a puttying-free and painting-free powdery coating as well as a preparation method and a use method thereof. The puttying-free and painting-free powdery coating comprises the following raw materials in parts by weight: 380-420 parts of high-alumina white cement, 3-4 parts of cellulose, 2-3 parts of bentonite, 0.4-0.6 part of an early strength agent, 18-22 parts of latex powder, 90-110 parts of coarse whiting and 450-500 parts of colored sand. The weakly-alkaline high-alumina white cement is used as a binder and occupies a large mass ratio, and the latex powder is used as the binder, so that the cohesiveness of a product can be greatly improved, the hardness of a paint film can be improved, the product can be directly formed in a batch scraping manner, puttying and roll coating of primer are not needed, and formaldehyde, methylbenzene and voc are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention discloses a powdery coating which is free from scraping putty and brushing paint, a preparation method and a use method thereof, and belongs to the field of coatings. Background Art

[0002] There are many non-toxic (zero formaldehyde, zero toluene, zero VOC, odorless) powder coatings in the prior art, such as an exterior wall putty powder and a preparation method thereof with publication number: CN110724404B, which comprises 300-400 parts of heavy calcium, 250-350 parts of white cement, 350-500 parts of quartz sand, 12-30 parts of latex powder, 4-5 parts of cellulose ether, 0.1-2 parts of starch ether, 1-3 parts of magnesium aluminum silicate, 1-2 parts of polyvinyl alcohol, 3-5 parts of pregelatinized starch, 1-5 parts of wood fiber, 3-5 parts of lime powder and 5-10 parts of rubber balls.

[0003] This technology uses heavy calcium, an inorganic mineral, as the main filling material. However, its viscosity is poor during use, and it is necessary to apply two coats of putty, then a primer and two coats of topcoat, which is time-consuming and labor-intensive. Summary of the invention

[0004] In view of the deficiencies in the prior art, the present invention aims to provide a powdered coating that does not require scraping, puttying or painting, and a preparation method and a use method thereof, so as to solve the problems.

[0005] In order to achieve the above-mentioned purpose, the present invention is realized through the following technical scheme: a powder coating that does not require scraping, puttying or painting, comprising the following raw materials in parts by weight: 380 to 420 parts of high-alumina white cement, 3 to 4 parts of cellulose, 2 to 3 parts of bentonite, 0.4 to 0.6 parts of early strength agent, 18 to 22 parts of latex powder, 90 to 110 parts of heavy calcium, and 450 to 500 parts of colored sand.

[0006] Preferably, the pH value of the high alumina white cement is 8-9.

[0007] Preferably, the cellulose is 100,000 viscosity cellulose.

[0008] Preferably, the heavy calcium is selected from 380 to 400 meshes.

[0009] Preferably, the colored sand includes 280 to 320 parts by weight of the first colored sand of 40 to 80 mesh and 170 to 180 parts by weight of the second colored sand of 90 to 120 mesh.

[0010] A method for preparing a powdered coating that does not require scraping, puttying or painting, comprising the following steps:

[0011] Step 1: Add high-alumina white cement into the mixing kettle and continue stirring until it is loose, as a binder;

[0012] Step 2: Add cellulose, bentonite, early strength agent and latex powder to the binder simultaneously or in a distributed manner and stir. Adjust the viscosity of the binder, add latex powder and stir to enhance the viscosity of the binder;

[0013] Step 3: Make the finished product, add heavy calcium and colored sand, and stir until it is fully mixed with the binder.

[0014] Preferably, the mixing kettle is a zero-gravity mixer.

[0015] Preferably, the mixing kettle is maintained at a rotation speed of 100 to 120 rpm.

[0016] Beneficial Effects

[0017] The present invention uses weakly alkaline high-aluminum white cement as a binder, which occupies a large mass ratio, and is supplemented with latex powder as a binder, which can greatly increase the adhesion of the product and the hardness of the paint film, so that the product can be directly scraped and formed without the need for scraping putty and rolling primer, and has zero formaldehyde, zero toluene, and zero VOC. BRIEF DESCRIPTION OF THE DRAWINGS

[0018] Other features, objects and advantages of the present invention will become more apparent from the detailed description of non-limiting embodiments made with reference to the following drawings:

[0019] Figure 1 This is a schematic diagram of a powder coating of the present invention that does not require scraping, puttying or painting; DETAILED DESCRIPTION

[0020] In order to make the technical means, creative features, objectives and effects achieved by the present invention easy to understand, the present invention is further explained below in conjunction with specific implementation methods.

[0021] Example 1

[0022] Step 1: Add 380 parts of high-aluminum white cement into the mixing kettle, and start the weightless mixer used as the mixing kettle to stir the high-aluminum white cement at a uniform speed of 100 rpm for 2 minutes to make the high-aluminum white cement in a loose state to serve as a binder;

[0023] Step 2: Add cellulose, bentonite, early strength agent and latex powder to the binder at the same time and stir for 2 minutes.

[0024] Step 3: After the finished product is made, add 90 parts of 380-mesh heavy calcium and 280 parts of 40-mesh first colored sand and 170 parts of 90-mesh second colored sand, and stir for 5 minutes until it is fully mixed with the binder.

[0025] The high-alumina white cement is weakly alkaline with a pH value of 8; and the added colored sand has color, so that the processed finished product has color.

[0026] Example 2

[0027] The difference from Example 1 is that the high-alumina white cement is increased to 400 parts, the latex powder is increased to 20 parts, the heavy calcium cement is increased to 100 parts, and the mesh size of the heavy calcium cement is changed to 400 meshes.

[0028] Example 3

[0029] The difference from Example 1 is that the high-alumina white cement is increased to 420 parts, the latex powder is increased to 22 parts, the heavy calcium cement is increased to 110 parts, and the mesh size of the heavy calcium cement is changed to 400 meshes.

[0030] The products obtained in Examples 1-3 were sent for inspection, and part of the inspection reports are shown in Table 1 below:

[0031] Table 1

[0032]

[0033]

[0034]

[0035] Comparative Example 1

[0036] The difference from Example 1 is that the high-alumina white cement is increased to 450 parts.

[0037] Comparative Example 2

[0038] The difference from Example 1 is that the high-alumina white cement is reduced to 350 parts.

[0039] Comparative Example 3

[0040] The difference from Example 1 is that the amount of heavy calcium is increased to 120 parts.

[0041] Comparative Example 4

[0042] The difference from Example 1 is that the heavy calcium is reduced to 80 parts.

[0043] This product uses colored sand, high-aluminum white cement, and heavy calcium as the main materials, among which the mass proportion of high-aluminum white cement is much greater than that of heavy calcium, so that in the preparation process of the powdered coating, high-aluminum white cement, as the main binder component, can provide a more stable structural foundation. Specifically, the dosage of high-aluminum white cement ranges from 380 to 420 parts, accounting for a large proportion of the overall raw materials, while the dosage of heavy calcium is 90 to 110 parts, which is relatively small. This ratio design not only enhances the bonding strength and durability of the coating, but also ensures the flatness and stability of the coating after construction. The high proportion of high-aluminum white cement enables the coating to form a solid coating on the wall or other substrates, effectively avoiding the problems of shedding and cracking that may occur during the process of part of the putty or painting, thereby achieving the effect of free scraping putty and free painting. Further testing shows that the proportion of high-aluminum white cement in comparative example 1 is too high, resulting in poor adhesion of the putty, easy cracking after drying, and shortened drying time, resulting in poor matching during subsequent application. In Comparative Example 2, the proportion of high-alumina white cement is too low, which reduces the filling capacity of the putty, resulting in a decrease in hardness and insufficient strength.

[0044] The proper addition of heavy calcium helps to adjust the performance and cost of the coating, so that the coating has a certain economy and environmental protection while maintaining excellent performance. Further testing shows that in Comparative Example 3, the heavy calcium is in too high a proportion. Similarly, this makes the adhesion of the putty poor, and it is easy to crack after drying, resulting in a decrease in strength. In Comparative Example 3, the heavy calcium is in too low a proportion, and the filling capacity of the putty is reduced, resulting in a decrease in hardness and insufficient strength.

[0045] Among them, weak alkaline high-alumina white cement is used as a binder, which can play a bonding role and increase the hardness of the paint film; while heavy calcium stone powder and Tiantan colored sand are used as inorganic minerals to have good filling properties and rich colors.

[0046] Selecting high-performance dispersible latex powder with good water resistance as an auxiliary agent can assist the high-alumina white cement with a large proportion to increase adhesion and crack resistance;

[0047] Selecting high molecular weight cellulose as a water-retaining agent; selecting bentonite as a lubricating agent can make the scraping smooth and prevent dripping after scraping.

[0048] A method for using a powdered coating that does not require scraping, puttying or painting.

[0049] Step S1: The finished product obtained in Example 1 is prepared according to the sample preparation ratio: powder: water = 1:0.5 (mass ratio);

[0050] Step S2: Stir the prepared materials to fully mix them.

[0051] Step S3: directly apply the paint obtained in step S2 to the wall, and apply twice.

[0052] In Example 4, 1.5 kg of the powdered paint prepared in this solution is preferably used per square meter of wall surface, and then 0.75 kg of tap water is added and stirred for 3 minutes to fully mix the two, and then the powdered paint is directly applied to the wall using existing tools. Furthermore, the total thickness of the two coatings is 1 mm; the product can be directly scraped and formed without the need for scraping putty and rolling primer.

[0053] The above shows and describes the basic principles and main features of the present invention and the advantages of the present invention. It is obvious to those skilled in the art that the present invention is not limited to the details of the above exemplary embodiments, and the present invention can be implemented in other specific forms without departing from the spirit or basic features of the present invention. Therefore, no matter from which point of view, the embodiments should be regarded as exemplary and non-restrictive. The scope of the present invention is defined by the attached claims rather than the above description, and it is intended that all changes falling within the meaning and scope of the equivalent elements of the claims are included in the present invention. Any figure mark in the claims should not be regarded as limiting the claims involved.

[0054] In addition, it should be understood that although the present specification is described according to implementation modes, not every implementation mode contains only one independent technical solution. This description of the specification is only for the sake of clarity. Those skilled in the art should regard the specification as a whole. The technical solutions in each embodiment may also be appropriately combined to form other implementation modes that can be understood by those skilled in the art.

Claims

1. A powder coating that does not require scraping, puttying or painting, characterized in that: The invention comprises the following raw materials in parts by weight: 380-420 parts of high-alumina white cement, 3-4 parts of cellulose, 2-3 parts of bentonite, 0.4-0.6 parts of early strength agent, 18-22 parts of latex powder, 90-110 parts of heavy calcium and 450-500 parts of colored sand.

2. The powder coating for scraping-free putty and painting-free according to claim 1, characterized in that: The pH value of the high-alumina white cement is 8-9.

3. The powdery coating for scraping-free putty and painting-free according to claim 1, characterized in that: The cellulose is 100,000 viscosity cellulose.

4. The powdery coating for scraping-free putty and painting-free according to claim 1, characterized in that: The heavy calcium is selected from 380 to 400 meshes.

5. The powdery coating for scraping-free putty and painting-free according to claim 1, characterized in that: The colored sand includes 40-80 meshes with a weight ratio of 280-320 parts of the first colored sand and 90-120 meshes with a weight ratio of 170-180 parts of the second colored sand.

6. A method for preparing a powdered coating that does not require scraping, puttying or painting, characterized in that: The following steps are involved: Step 1: Add high-alumina white cement into the mixing kettle and continue stirring until it is loose to serve as a binder; Step 2: Add cellulose, bentonite, early strength agent and latex powder into the binder simultaneously or in a distributed manner and stir. Step 3; To make the finished product, add heavy calcium and colored sand and stir until it is fully mixed with the binder.

7. The method for preparing a powdered coating for scraping-free putty and painting-free according to claim 6, characterized in that: The mixing kettle is a zero-gravity mixer.

8. The method for preparing a powdered coating for scraping-free putty and painting-free according to claim 7, characterized in that: The stirring kettle is maintained at a rotation speed of 100 to 120 rpm.

9. A method for using a powdered coating that does not require scraping, puttying or painting, characterized in that: The following steps are involved: Step S1: Mix the powdered coating according to the sample preparation ratio: powder: water = 1:0.5 (mass ratio); Step S2: Stir the prepared materials to fully mix them. Step S3: directly apply the paint obtained in step S2 to the wall, and apply twice.

Citation Information

Patent Citations

  • An exterior wall putty powder and its preparation method

    CN110724404B

  • Industrial bearing cement based self-leveling material

    CN102190462A

  • Self-leveling waterproof mortar of imitated stone facing and construction process of waterproof mortar

    CN103936370A

  • Method for decorating building wall through wall paint and waterproof anti-crack mortar

    CN104790606A

  • Single-component high-strength impervious thin layer repair mortar as well as preparation method and application thereof

    CN113004015A