Application of retinoic acid / hydromagnesite composite powder in detection of micro-area viscosity of correction fluid

Through the use of retinoic acid/water magnesium compound powder, the problems of coating liquid in covering force, flame retardant and micro-zone viscosity detection are solved, and efficient coating liquid development and application are realized, and visual detection tools are provided. Low-cost industrialized solutions.

CN119081466APending Publication Date: 2024-12-06JIANGXI HONGYI POLYMERIC MATERIALS +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411210937.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2023-05-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The existing coating liquid has shortcomings in terms of hiding strength and flame retardant effects, and it is difficult to visually detect micro-zone viscosity, which affects its efficient development and application.

Method used

Retinoic acid/water magnesite composite powder is used, which consists of retinoic acid and water magnesite, and is prepared by dehydration and condensation reaction. Retinoic acid is used as the shell and water magnesite is used as the core, and the molar ratio is 1 to 50. :1. It has a flexible conjugated structure and high whiteness, which can release light signals in different viscosity environments, assist in detection and flame retardant.

Benefits of technology

It realizes the high hiding force, flame retardant effect and micro-zone viscosity detection of the modification liquid, provides visual formulation design tools, reduces costs, and is suitable for large-scale industrial applications.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081466A_ABST
    Figure CN119081466A_ABST
Patent Text Reader

Abstract

The invention provides application of retinoic acid / hydromagnesite composite powder in detection of correction fluid microcell viscosity, and belongs to the technical field of photochemical detection. The retinoic acid / hydromagnesite composite powder is composed of retinoic acid and hydromagnesite, the retinoic acid serves as a shell of the composite powder, the hydromagnesite serves as an inner core of the composite powder, and the molar ratio of the retinoic acid to the hydromagnesite is 100: 4. The retinoic acid / hydromagnesite composite powder is prepared by sequentially mixing a hydromagnesite solution and a dehydrating agent dispersion liquid with a retinoic acid solution and then carrying out a dehydration condensation reaction. The retinoic acid / hydromagnesite composite powder disclosed by the invention can release weak light signals in a low-viscosity correction fluid and release strong light signals in a high-viscosity correction fluid, so that the formula design of the correction fluid is facilitated. Moreover, due to the conjugated structure of the retinoic acid, the retinoic acid can be easily charred in the combustion process, and the retinoic acid and the internal hydromagnesite have a better synergistic flame-retardant effect.
Need to check novelty before this filing date? Find Prior Art

Description

[0001] This application is a divisional application. The application number of the parent application is 202310594588.7, the application date is May 24, 2023, and the name of the invention is "A retinoic acid / hydromagnesium composite powder and its preparation method and application". Technical Field

[0002] The invention relates to the technical field of photochemical detection, and in particular to the application of retinoic acid / hydromagnesium composite powder in detecting the viscosity of correction fluid micro-regions. Background Art

[0003] Correction fluid is a white opaque pigment used to cover typos and can be written repeatedly. It is widely used in various types of stationery paperwork, and its correction effect has been deeply rooted in people's hearts. It mainly contains many ingredients such as trichloroethane, methylcyclohexane, cyclohexane, etc., and also contains inorganic powders such as calcium carbonate that provide hiding power. It usually needs to be used up within a period of time during daily use, because long-term storage can cause internal solvents and fillers to stratify, and the solvent is more volatile, which can easily cause the correction fluid to become viscous. Not only that, as an emulsion, the amount of solvent added during the preparation process will also profoundly affect the correction effect of the correction fluid. This is all related to its viscosity. If the viscosity is too low, the fluidity will increase, but it will easily lead to it being too thin when brushed, and the hiding power will decrease; on the contrary, if the viscosity is too high, the fluidity will decrease and it will be too thick when brushed, and the hiding power will increase to a certain extent, but at this time the solid content is relatively high, and the cost will increase. Therefore, it is necessary to develop a functional material that is fast, convenient, and visual for detecting the viscosity of correction fluid, which even has certain covering properties. It can sense the viscosity changes by the release strength of the light signal, which can make the efficient development and application of correction fluid have important practical significance.

[0004] Generally, in addition to adding inorganic powders to meet the most basic hiding power, correction fluids need to add some flame retardants to avoid accidental combustion caused by uncontrollable factors during storage and use. From another perspective, correction fluids also have high requirements for micro-area viscosity during preparation. Most existing analytical detection methods are strongly dependent on equipment, and usually measure macroscopic viscosity, which makes it difficult to visualize imaging at the molecular level. In contrast, photochemical analysis technology that integrates natural product functional organic molecules has significant advantages in detection sensitivity, imaging timeliness, and ease of operation, especially for micro-area viscosity changes. The response is relatively sensitive. Loading various types of photochemical functional sensors on inorganic powders has further developed into a powder platform with multiple capabilities, which has become one of the core means to solve the above problems in recent years. Therefore, it is urgent to develop multifunctional composite powders that can simultaneously meet the requirements of good hiding power, flame retardant effect and micro-area viscosity measurement. This strategy has become a trend in improving the high-value application of traditional inorganic powders. Summary of the invention

[0005] The purpose of the present invention is to provide a retinoic acid / hydromagnesium composite powder and a preparation method and application thereof, so as to solve the technical problems in the prior art that the correction fluid has poor hiding power and flame retardant effect and micro-area viscosity detection cannot be visualized.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The invention provides a retinoic acid / hydromagnesium composite powder, which consists of retinoic acid and hydromagnesium, wherein the retinoic acid is the outer shell of the composite powder and the hydromagnesium is the inner core of the composite powder; the molar ratio of the retinoic acid to the hydromagnesium is 1-50:1.

[0008] Preferably, the D of the retinoic acid / hydromagnesium composite powder is 50 0.9~3.0μm, among which the D 50 0.8~2.8μm.

[0009] The invention provides a method for preparing a retinoic acid / hydromagnesium composite powder, comprising the following steps: mixing a hydromagnesium solution and a dehydrating agent dispersion with a retinoic acid solution in sequence, and then performing a dehydration condensation reaction to obtain the retinoic acid / hydromagnesium composite powder.

[0010] Preferably, the retinoic acid solution is formed by mixing retinoic acid and a solvent; the hydromagnesium solution is formed by mixing hydromagnesium and a solvent; the dehydrating agent dispersion is formed by mixing a dehydrating agent and a solvent; and the solvent independently comprises one or more of ethanol, methanol, tetrahydrofuran, N,N-dimethylformamide, dimethyl sulfoxide, acetonitrile, water and ethyl acetate.

[0011] Preferably, the concentration of the retinoic acid solution is 1-500 mol / L; the concentration of the hydromagnesia solution is 1-4 mol / L; and the content of the dehydrating agent in the dehydrating agent dispersion is 1-1000 mol / L.

[0012] Preferably, the dehydrating agent comprises K 2 CO 3 , Cs 2 CO 3 、CaCO 3 、Na 2 CO 3 、NaHCO 3 and Ca(OH) 2 One of;

[0013] The molar ratio of the dehydrating agent to hydromagnesite is 1 to 1000:1.

[0014] Preferably, the temperature of the dehydration condensation reaction is 45 to 100° C., and the time of the dehydration condensation reaction is 1 to 60 hours.

[0015] Preferably, the product of the dehydration condensation reaction is sequentially filtered, precipitated, centrifuged and freeze-dried; the freeze-drying temperature is -70 to -5°C, and the freeze-drying time is 1 to 96 hours.

[0016] The invention provides an application of a retinoic acid / hydromagnesium composite powder in correction fluid. The retinoic acid / hydromagnesium composite powder is mixed with the correction fluid.

[0017] Preferably, the mixing concentration of the retinoic acid / hydromagnesium composite powder is 0.1-20 μmol / L.

[0018] The retinoic acid / hydromagnesium composite powder provided by the present invention is prepared by combining the natural product retinoic acid and the natural magnesium salt through chemical bonds to form an organic-inorganic multifunctional composite powder (such as Figure 1 As shown). The functionalized composite powder is added to correction fluids of different viscosities. The retinoic acid on its surface can rotate freely in a low-viscosity solution environment because it has multiple flexible conjugated structures that can rotate freely. The excited energy can be consumed by mechanical dissipation, showing a non-radiative transition, so that the released light signal is weak or even disappears. In a high-viscosity correction fluid environment, its free rotation is restricted, so that the channel that originally returns to the ground state through non-radiative transition is closed, and it returns to the ground state through radiative transition, thereby releasing a strong fluorescence signal. This phenomenon is closely related to the physical viscosity of the correction fluid itself. The strength of the released light signal can assist in judging the consistency of the correction fluid formula design. This design can realize visual tracking of the formulas of different correction fluids (the specific detection mechanism is as shown in Figure 3 As shown); Moreover, hydromagnesite itself has a high whiteness, and it is basic magnesium carbonate, which is a composite of magnesium carbonate and magnesium hydroxide, and has natural advantages in flame retardancy and smoke suppression.

[0019] Beneficial effects of the present invention:

[0020] (1) The present invention uses hydromagnesite powder, which is widely found in nature, as the main body of the functional material. Hydromagnesite powder has a high whiteness and good flame retardant and smoke suppression properties, which can meet the hiding power and flame retardant requirements of inorganic powders of correction fluid. Most importantly, it comes from nature and can be obtained as ultrafine powder by physical grinding and graded air separation;

[0021] (2) The retinoic acid / hydromagnesium composite powder provided by the present invention has a layer of retinoic acid on its surface. This substance is one of the retinol substances commonly found in nature and has a flexible conjugated structure. It can release weak light signals in low-viscosity correction fluids and strong light signals in high-viscosity correction fluids, which is helpful for the formulation design of correction fluids and greatly expands the application scenarios of natural products in many environments.

[0022] (3) The shell retinoic acid on the surface of the retinoic acid / hydromagnesium composite powder provided by the present invention has a large number of conjugated structures, which makes it very easy to form carbon during the combustion process. It is a typical natural carbon-forming agent, which can improve the flame retardant properties of the composite powder and provide a physical shielding layer in the condensed phase to suppress the impact of air flow, mass flow and heat flow, and has a good synergistic flame retardant effect with the internal hydromagnesium;

[0023] (4) The retinoic acid / hydromagnesium composite powder provided by the present invention can be prepared by a one-step method, the preparation process is simple, the main raw materials used are all from nature, they are typical natural products, very environmentally friendly, easy to carry out chemical design and can be mass-produced, suitable for large-scale industrial application, and at the same time, there is no complicated post-processing process, the price is relatively low, and the comprehensive application cost is low. BRIEF DESCRIPTION OF THE DRAWINGS

[0024] Figure 1 Schematic diagram of the structure of the retinoic acid / hydromagnesium composite powder prepared in Examples 1 to 3;

[0025] Figure 2 This is a SEM image of the retinoic acid / hydromagnesium composite powder prepared in Example 1;

[0026] Figure 3 Schematic diagram of the induction mechanism of the retinoic acid / hydromagnesium composite powder prepared in Examples 1 to 3 to low-viscosity and high-viscosity correction fluids;

[0027] Figure 4 Spectra of the retinoic acid / hydromagnesium composite powder prepared in Example 1 in solutions with different viscosities;

[0028] Figure 5 The linear fitting graph of the logarithmic function of the fluorescence intensity and solution viscosity of the retinoic acid / hydromagnesium composite powder prepared in Example 1;

[0029] Figure 6 The absorption spectra of the retinoic acid / hydromagnesium composite powder prepared in Example 1 in solutions of different polarities;

[0030] Figure 7 This is a light stability test chart of the retinoic acid / hydromagnesium composite powder prepared in Example 1;

[0031] Figure 8This is the optical signal release spectrum of the retinoic acid / hydromagnesium composite powder prepared in Example 1 in different viscosity correction slurries. DETAILED DESCRIPTION

[0032] The hydromagnesite powder used in the present invention is prepared by physical grinding, generally by multiple ball milling and wind classification to select the hydromagnesite powder with a suitable particle size.

[0033] The invention provides a retinoic acid / hydromagnesium composite powder, which consists of retinoic acid and hydromagnesium, wherein the retinoic acid is the outer shell of the composite powder and the hydromagnesium is the inner core of the composite powder; the molar ratio of the retinoic acid to the hydromagnesium is 1-50:1.

[0034] In the present invention, the retinoic acid is a naturally occurring organic small molecule, and its specific chemical structure is shown in Formula I. Its full name is 3,7-dimethyl-9-(2,6,6-trimethylcyclohex-1-en-1-yl)nona-2,4,6,8-tetraenoic acid, abbreviated as DTCT, and its molecular formula is C 20 H 28 O 2 , the relative molecular mass is 300.20.

[0035]

[0036] In the present invention, the molar ratio of retinoic acid to hydromagnesium is preferably 2 to 45:1, and more preferably 4 to 40:1.

[0037] In the present invention, when the molar ratio of retinoic acid to hydromagnesia is lower than 1:1, the content of surface retinoic acid is relatively low, and the composite effect on hydromagnesia is limited. Both the viscosity sensing measurement and the flame retardant effect may be low, and the comprehensive performance is reduced. On the other hand, when the molar ratio of retinoic acid to hydromagnesia is greater than 50:1, the concentration of surface retinoic acid may be too high, and excessive retinoic acid may wrap multiple hydromagnesia particles together, which may cause the hydromagnesia particles to be larger, which has a greater impact on the final hiding power improvement, flame retardant effect and viscosity response during the preparation process.

[0038] In the present invention, the D of the retinoic acid / hydromagnesium composite powder is 50 is 0.9 to 3.0 μm, preferably 1.0 to 2.8 μm, and more preferably 1.2 to 2.6 μm; wherein the D 50 The thickness is 0.8 to 2.8 μm, preferably 1.2 to 2.6 μm, and more preferably 1.4 to 2.4 μm.

[0039] The invention provides a method for preparing a retinoic acid / hydromagnesium composite powder, comprising the following steps: mixing a hydromagnesium solution and a dehydrating agent dispersion with a retinoic acid solution in sequence, and then performing a dehydration condensation reaction to obtain the retinoic acid / hydromagnesium composite powder.

[0040] In the present invention, the process of the dehydration condensation reaction is as follows:

[0041]

[0042] In the present invention, the retinoic acid solution is formed by mixing retinoic acid and a solvent; the hydromagnesium solution is formed by mixing hydromagnesium and a solvent; the dehydrating agent dispersion is formed by mixing a dehydrating agent and a solvent; the solvent independently comprises one or more of ethanol, methanol, tetrahydrofuran, N,N-dimethylformamide, dimethyl sulfoxide, acetonitrile, water and ethyl acetate, preferably one or more of ethanol, methanol, tetrahydrofuran, N,N-dimethylformamide and dimethyl sulfoxide, and further preferably one or more of ethanol, tetrahydrofuran and N,N-dimethylformamide.

[0043] In the present invention, the retinoic acid solution is preferably prepared under stirring conditions, wherein the stirring rate is 100-900 rpm, preferably 200-800 rpm, and more preferably 300-700 rpm; the stirring temperature is 20-45°C, preferably 25-40°C, and more preferably 30-35°C; the stirring time is 10-150 min, preferably 30-130 min, and more preferably 50-100 min.

[0044] In the present invention, the hydromagnesite solution is preferably prepared under stirring conditions, wherein the stirring rate is 100-1300 rpm, preferably 200-1200 rpm, and more preferably 400-1000 rpm; the stirring temperature is 20-50° C., preferably 25-45° C., and more preferably 30-40° C.; the stirring time is 10-300 min, preferably 40-270 min, and more preferably 60-240 min.

[0045] In the present invention, the hydromagnesium solution and the retinoic acid solution are preferably mixed by dropwise addition, wherein the dropwise addition rate is 1 drop / s to 1 drop / 10s, preferably 1 drop / 2s to 1 drop / 8s, and more preferably 1 drop / 3s to 1 drop / 5s.

[0046] In the present invention, the concentration of the retinoic acid solution is 1 to 500 mol / L, preferably 2 to 400 mol / L, and more preferably 5 to 350 mol / L; the concentration of the hydromagnesia solution is 1 to 4 mol / L, preferably 1.5 to 3.5 mol / L, and more preferably 2 to 3 mol / L; the content of the dehydrating agent in the dehydrating agent dispersion is 1 to 1000 mol / L, preferably 10 to 900 mol / L, and more preferably 20 to 800 mol / L.

[0047] In the present invention, the dehydrating agent comprises K 2 CO 3 , Cs 2 CO 3 、CaCO 3 、Na 2 CO 3 、NaHCO 3 and Ca(OH) 2 One of the following, preferably K 2 CO 3 , Cs 2 CO 3 、Na 2 CO 3 and NaHCO 3 One or more of, more preferably K 2 CO 3 , Cs 2 CO 3 and Na 2 CO 3 One or more of the .

[0048] In the present invention, the molar ratio of the dehydrating agent to hydromagnesite is 1 to 1000:1, preferably 2 to 900:1, and more preferably 4 to 800:1.

[0049] In the present invention, the temperature of the dehydration condensation reaction is 45 to 100° C., preferably 50 to 90° C., and more preferably 60 to 80° C.; the time of the dehydration condensation reaction is 1 to 60 h, preferably 5 to 55 h, and more preferably 10 to 50 h.

[0050] In the present invention, the dehydration condensation reaction is carried out under stirring conditions, wherein the stirring rate is 100 to 1500 rpm, preferably 200 to 1300 rpm, and more preferably 300 to 1100 rpm.

[0051] In the present invention, the product of the dehydration condensation reaction is sequentially subjected to suction filtration precipitation, centrifugal washing and freeze drying.

[0052] In the present invention, the suction filtration and precipitation are carried out in two steps, the first step is suction filtration, and the second step is precipitation. The suction filtration is to filter the liquid after the dehydration condensation reaction is completed, wherein a fast or medium-speed filter paper is used in the suction filtration process, and the vacuum degree is controlled to be -0.098 to -0.07MPa, preferably -0.09 to -0.075MPa, and more preferably -0.085 to -0.08MPa, and the suction filtration is repeatedly rinsed with a solvent during the suction filtration process, and the solvent is one or more mixed solutions of methanol, ethanol and deionized water, preferably methanol and / or ethanol, and more preferably ethanol; the precipitation is to redisperse the solid powder after suction filtration in ethanol, and then let it stand and precipitate, and remove the upper clear liquid, wherein the time for standing and settling is 1 to 48 hours, preferably 5 to 40 hours, and more preferably 10 to 35 hours.

[0053] In the present invention, the centrifugal washing is to add deionized water to the solid product precipitated by suction filtration for multiple times, and the solid content of the solid product in the deionized water is controlled to be 1 to 20 g / mL, preferably 3 to 18 g / mL, and more preferably 5 to 15 g / mL; the centrifugal rate is 1000 to 10000 rpm, preferably 1500 to 9000 rpm, and more preferably 2000 to 7000 rpm; the centrifugal time is 3 to 60 min, preferably 10 to 50 min, and more preferably 20 to 40 min.

[0054] In the present invention, the freeze-drying temperature is -70 to -5°C, preferably -65 to -10°C, and more preferably -55 to -15°C; the freeze-drying time is 1 to 96 hours, preferably 5 to 90 hours, and more preferably 10 to 80 hours.

[0055] The invention provides an application of a retinoic acid / hydromagnesium composite powder in correction fluid. The retinoic acid / hydromagnesium composite powder is mixed with the correction fluid.

[0056] In the present invention, the mixing concentration of the retinoic acid / hydromagnesium composite powder is 0.1 to 20 μmol / L, preferably 1 to 18 μmol / L, and more preferably 5 to 15 μmol / L.

[0057] In the present invention, when the retinoic acid / hydromagnesium composite powder and the correction fluid are mixed, it is preferably carried out under stirring conditions, wherein the stirring rate is 50 to 500 rpm, preferably 100 to 400 rpm, and more preferably 150 to 350 rpm; the stirring temperature is 20 to 45°C, preferably 25 to 40°C, and more preferably 30 to 35°C; the stirring time is 1 to 12 hours, preferably 2 to 10 hours, and more preferably 4 to 8 hours.

[0058] The retinoic acid / hydromagnesia composite powder provided by the present invention is applied to correction fluid, which can not only provide good hiding power, but also has good flame retardant properties, and can effectively improve the combustion inhibition properties of the correction fluid. Moreover, during the preparation process, the micro-region viscosity, a key physical indicator, can be detected and imaged, providing a useful reference for the formulation design of the correction fluid. Based on this, the retinoic acid / hydromagnesia composite powder is a multi-purpose functionalized powder further realized on the basis of traditional hydromagnesia powder.

[0059] The technical solutions provided by the present invention are described in detail below in conjunction with the embodiments, but they should not be construed as limiting the protection scope of the present invention.

[0060] In the present invention, the D of the hydromagnesite powder used in Examples 1 to 3 and Comparative Examples 1 to 2 is 50 It is 2.8μm.

[0061] Example 1

[0062] Dissolve 100 mol of retinoic acid in N,N-dimethylformamide, stir at 400 rpm for 80 min at 25°C to obtain a retinoic acid solution with a concentration of 100 mol / L; disperse 4 mol of hydromagnesia powder in N,N-dimethylformamide, stir at 800 rpm for 120 min at 30°C to obtain a hydromagnesia solution with a concentration of 4 mol / L. Then add the hydromagnesia solution dropwise to the retinoic acid solution at a rate of 1 drop / 5s. After the addition is complete, add 1 L of K 2 CO 3 The dispersion is added to the above mixed solution, wherein K 2 CO 3 The dispersion is composed of K 2 CO 3 and N,N-dimethylformamide, K 2 CO 3The content is 100 mol / L, and a dehydration condensation reaction is carried out at 60°C. The stirring rate during the reaction is 1000 rpm, and the reaction time is controlled to be 24 hours. After the reaction is completed, the reaction product is filtered and precipitated, centrifuged and washed, and freeze-dried in sequence. The specific steps are: a fast filter paper is used during the filtration process, and the vacuum degree is controlled to be -0.098 MPa. The filtration process is repeated with ethanol to wash the filtration several times; the solid powder after filtration is redispersed in ethanol, allowed to settle for 12 hours, and the upper clear liquid is removed; the solid powder after filtration and precipitation is dispersed in deionized water, wherein the solid content of the solid powder in the deionized water is 10 g / mL, and then placed in a centrifuge for centrifugal washing, the centrifugal rate used is 6000 rpm, and the centrifugal time is 30 minutes; after centrifugal washing three times, the solid powder is placed in a low-temperature dryer for freeze drying, wherein the freeze drying temperature is -45°C, and the freeze drying time is 32 hours, and retinoic acid / hydromagnesium composite powder can be obtained.

[0063] Figure 2 This is the SEM image of the retinoic acid / hydromagnesium composite powder prepared in Example 1. Figure 2 It can be seen that there are a variety of granular substances attached to the surface of the hydromagnesite powder on the surface of the composite powder. The surface is relatively rough but continuous and dense. The edges of each particle are clear and relatively independent, and it has a good coating effect (as shown in the circle in the figure).

[0064] Example 2

[0065] Dissolve 1 mol of retinoic acid in ethanol and stir at 100 rpm for 150 min at 20°C to obtain a retinoic acid solution with a concentration of 1 mol / L. Disperse 1 mol of hydromagnesia powder in ethanol and stir at 100 rpm for 30 min at 20°C to obtain a hydromagnesia solution with a concentration of 1 mol / L. Then add the hydromagnesia solution dropwise to the retinoic acid solution at a rate of 1 drop / 10 s. After the addition is complete, add 1 L of Cs 2 CO 3 The dispersion is added to the above mixed solution, wherein Cs 2 CO 3 The dispersion is composed of Cs 2 CO 3 and ethanol, Cs 2 CO 3The content of is 100 mol / L, and a dehydration condensation reaction is carried out at 45°C. The stirring rate during the reaction is 1500 rpm, and the reaction time is controlled to be 60 hours. After the reaction is completed, the reaction product is filtered and precipitated, centrifuged and washed, and freeze-dried in sequence. The specific steps are: a fast filter paper is used during the filtration process, and the vacuum degree is controlled to be -0.07 MPa. The filtration process is repeated with ethanol to wash the filtration several times; the solid powder after filtration is redispersed in ethanol, and the precipitated solid powder is allowed to stand for 48 hours, and the supernatant is removed; the solid powder after filtration and precipitation is dispersed in deionized water, wherein the solid content of the solid powder in the deionized water is 1 g / mL, and then placed in a centrifuge for centrifugal washing, the centrifugal rate used is 1000 rpm, and the centrifugal time is 60 minutes; after centrifugal washing three times, the solid powder is placed in a low-temperature dryer for freeze drying, wherein the freeze drying temperature is -70°C, and the freeze drying time is 1 hour, and retinoic acid / hydromagnesium composite powder can be obtained.

[0066] Example 3

[0067] Dissolve 100 mol of retinoic acid in dimethyl sulfoxide, stir at 900 rpm for 10 min at 45°C to obtain a retinoic acid solution with a concentration of 400 mol / L; disperse 2 mol of hydromagnesia powder in dimethyl sulfoxide, stir at 1300 rpm for 10 min at 50°C to obtain a hydromagnesia solution with a concentration of 2 mol / L. Then add the hydromagnesia solution dropwise to the retinoic acid solution at a rate of 1 drop / s. After the addition is complete, add 1 L of Na 2 CO 3 The dispersion was added to the above mixed solution, wherein Na 2 CO 3 The dispersion is composed of Na 2 CO 3 and ethanol, Na 2 CO 3The content of 1000mol / L is carried out at 100℃ for dehydration condensation reaction, the stirring rate during the reaction is 100rpm, and the reaction time is controlled to be 1h; after the reaction is completed, the reaction product is filtered and precipitated, centrifuged and washed, and freeze-dried in sequence, and the specific steps are: medium-speed filter paper is used during the filtration process, the vacuum degree is controlled to be -0.08MPa, and ethanol is used to repeatedly rinse the filtration process; the solid powder after filtration is redispersed in ethanol, allowed to settle for 1h, and the upper clear liquid is removed; the solid powder after filtration and precipitation is dispersed in deionized water, wherein the solid content of the solid powder in the deionized water is 10g / mL, and then placed in a centrifuge for centrifugal washing, the centrifugal rate used is 10000rpm, and the centrifugal time is 3min; after centrifugal washing four times, the solid powder is placed in a low-temperature dryer for freeze drying, wherein the freeze drying temperature is -75℃, and the freeze drying time is 96h, and retinoic acid / hydromagnesium composite powder can be obtained.

[0068] Comparative Example 1

[0069] 0.5 mol of retinoic acid was dissolved in N,N-dimethylformamide, and stirred at 600 rpm for 80 min at 35°C to obtain a retinoic acid solution with a concentration of 0.5 mol / L; 1 mol of hydromagnesia powder was dispersed in N,N-dimethylformamide, and stirred at 1000 rpm for 120 min at 40°C to obtain a hydromagnesia solution with a concentration of 1 mol / L. The hydromagnesia solution was then added dropwise to the retinoic acid solution at a rate of 1 drop / 3s. After the addition was completed, 1L of NaHCO 3 The dispersion was added to the above mixed solution, wherein NaHCO 3 The dispersion is composed of NaHCO 3 and N,N-dimethylformamide, Na 2 CO 3The content is 200 mol / L, and a dehydration condensation reaction is carried out at 70°C. The stirring rate during the reaction is 600 rpm, and the reaction time is controlled to be 18 hours. After the reaction is completed, the reaction product is filtered and precipitated, centrifuged and washed, and freeze-dried in sequence. The specific steps are: a fast filter paper is used during the filtration process, and the vacuum degree is controlled to be -0.08 MPa. The filtration process is repeated with ethanol to wash the filtration several times; the solid powder after filtration is redispersed in ethanol, allowed to settle for 1 hour, and the upper clear liquid is removed; the solid powder after filtration and precipitation is dispersed in deionized water, wherein the solid content of the solid powder in the deionized water is 8 g / mL, and then placed in a centrifuge for centrifugal washing, the centrifugal rate used is 5000 rpm, and the centrifugal time is 45 minutes; after four centrifugal washings, the solid powder is placed in a low-temperature dryer for freeze drying, wherein the freeze drying temperature is -25°C, and the freeze drying time is 72 hours, and retinoic acid / hydromagnesium composite powder can be obtained.

[0070] Comparative Example 2

[0071] 120 mol of retinoic acid was dissolved in N,N-dimethylformamide, and stirred at 600 rpm for 100 min at 25°C to obtain a retinoic acid solution with a concentration of 400 mol / L; 2 mol of hydromagnesia powder was dispersed in N,N-dimethylformamide, and stirred at 1100 rpm for 150 min at 30°C to obtain a hydromagnesia solution with a concentration of 2 mol / L. The hydromagnesia solution was then added dropwise to the retinoic acid solution at a rate of 1 drop / 2s. After the addition was completed, 2L of CaCO 3 The solution was added to the above mixed solution, wherein CaCO 3 The dispersion is composed of CaCO 3 and N,N-dimethylformamide, CaCO 3 The content is 300mol / L, and a dehydration condensation reaction is carried out at 80°C. The stirring rate during the reaction is 900rpm, and the reaction time is controlled to be 16h. After the reaction is completed, the reaction product is filtered and precipitated, centrifuged and washed, and freeze-dried in sequence. The specific steps are: a fast filter paper is used during the filtration process, and the vacuum degree is controlled to be -0.085MPa. The filtration process is repeated with ethanol to wash the filtration; the solid powder after filtration is redispersed in ethanol, allowed to settle for 30h, and the supernatant is removed; the solid powder after filtration and precipitation is dispersed in deionized water, wherein the solid content of the solid powder in the deionized water is 8g / mL, and then placed in a centrifuge for centrifugal washing, the centrifugal rate used is 3500rpm, and the centrifugal time is 55min; after four centrifugal washings, the solid powder is placed in a low-temperature dryer for freeze drying, wherein the freeze drying temperature is -55°C, and the freeze drying time is 36h, and retinoic acid / hydromagnesium composite powder can be obtained.

[0072] Performance Test:

[0073] The particle size, oil absorption value and specific surface area of ​​the retinoic acid / hydromagnesium composite powder prepared by the raw material hydromagnesium, Examples 1 to 3, and Comparative Examples 1 to 2 were tested. The test results are shown in Table 1.

[0074] The specific test methods are as follows: (1) Particle size: a laser particle distribution measuring instrument is used to measure the particle size and distribution of the powder; (2) Oil absorption value: the test is conducted in accordance with DB / T5211.15-2014 standard; (3) Specific surface area: the specific surface area BET is used for testing.

[0075] Table 1 Particle size, oil absorption value and specific surface area test results

[0076] project <![CDATA[D 50 (μm)]]> Oil absorption value (mL / 100g) <![CDATA[Specific surface area (m 2 / g) <!-- 7 -->]]> Hydromagnesite 2.8 60 10.02 Example 1 1.67 29 17.85 Example 2 1.69 30 17.62 Example 3 1.71 31 17.34 Comparative Example 1 2.88 50 12.13 Comparative Example 2 3.03 45 11.10

[0077] It can be seen from the test results of Examples 1 to 3 in Table 1 that after adding a certain proportion of natural product retinoic acid to modify hydromagnesium, the median particle size D 50 It shows a typical downward trend, indicating that retinoic acid-modified hydromagnesia can mostly appear in a state of single particle dispersion, which may be related to the fact that retinoic acid can well shield the hydroxyl groups on the surface of hydromagnesia, making it hydrophobic, and there are no other forces such as hydrogen bonds between them, thereby effectively reducing the agglomeration effect between powders. In contrast, when the surface retinoic acid is too little (the molar ratio is less than 1:1, such as in Comparative Example 1) or too high (the molar ratio is greater than 50:1, such as in Comparative Example 2), its modification effect on hydromagnesia is in a declining state, D 50The increase in the value indicates that a typical agglomeration phenomenon has occurred. From the perspective of oil absorption value, the addition of a suitable proportion of retinoic acid can significantly improve the oil absorption value of hydromagnesite powder, reducing it from the original 60mL / 100g to 29-31mL / 100g. This may be related to the hydrophobic structure of retinoic acid itself. The decrease in oil absorption value can significantly improve its adsorption performance of additives during processing, save costs, and help improve its fluidity during processing, thereby improving its overall performance. When the molar ratio of the added natural product retinoic acid to hydromagnesite is too low or too high, the oil absorption value of the composite powder will still increase. Although it has a certain downward trend compared to the oil absorption value of the completely unmodified hydromagnesite powder, the oil absorption The value is still high, which is not conducive to the improvement of the comprehensive performance of the composite powder; then, from the perspective of specific surface area, after modification with a suitable proportion of natural product retinoic acid, its specific surface area showed a significant improvement, with an improvement effect of nearly 78%, which may be related to the dispersion of the composite powder and the decrease in the median particle size. In contrast, when the addition amount of natural product retinoic acid is too low or too high, its specific surface area does not increase significantly. This may be due to the low molar ratio of the surface retinoic acid, which still leaves a lot of hydroxyl groups on its surface and is prone to agglomeration. Not only does the median particle size increase, but the specific surface area also decreases accordingly. When the molar ratio of the surface retinoic acid is high, it may wrap multiple hydromagnesite powder particles together, increasing the particle size and reducing the specific surface area. The above results show that the surface polarity of natural hydromagnesite can be effectively improved by adding a suitable proportion of natural product retinoic acid, which is beneficial to improving the comprehensive performance of the composite powder.

[0078] Spectroscopic testing of retinoic acid / hydromagnesium complex powder.

[0079] (1) Response test of retinoic acid / hydromagnesium composite powder in solutions with different viscosities:

[0080] Solutions of different viscosities were prepared by adding different volume fractions of glycerol to deionized water, and the retinoic acid / hydromagnesium composite powder prepared in Example 1 was added to the above solution, and allowed to stand for a period of time at room temperature, and the concentration of the added retinoic acid / hydromagnesium composite powder was controlled to be 10 μM, wherein the excitation wavelength was 410 nm, and the measured spectrum was as follows: Figure 4As shown. From the results, it can be seen that as the viscosity of the solution gradually increases, the intensity of the obtained fluorescence signal becomes more and more significant, indicating that the composite powder can have a good response effect on viscosity. This may be because a large amount of retinoic acid on the surface contains more freely rotatable conjugated structures. These conjugated single and double bonds can rotate freely in low-viscosity solutions and consume the energy of the excited state through mechanical dissipation. In high-viscosity solutions, it is difficult to rotate freely, and then the excited state energy is dissipated through radiation transition, releasing a strong fluorescence signal, which increases by about 65 times as a whole (as shown in Table 2). It can be seen that the composite powder has a good response effect on the micro-area viscosity of the solution. In addition, the present invention tested the sensitivity coefficient of the retinoic acid / hydromagnesium composite powder prepared in Example 1 to viscosity. Figure 5 The test results show that the viscosity sensitivity coefficient of the composite powder is 1.93, showing a strong application potential for viscosity enhancement of correction fluid.

[0081] Table 2 Light signal intensity of retinoic acid / hydromagnesium composite powder in different viscosity solution atmospheres

[0082]

[0083]

[0084] (2) Absorption spectra of retinoic acid / hydromagnesium composite powder in different polar solvents:

[0085] Correction fluid needs to add multiple solvents due to its multifunctional requirements. The signal stability of retinoic acid / hydromagnesium composite powder in multiple solvent systems is crucial. The retinoic acid / hydromagnesium composite powder prepared in Example 1 was added to six common solvents, namely water, ethanol, tetrahydrofuran, dimethyl sulfoxide, toluene, and glycerol. The concentration of retinoic acid / hydromagnesium composite powder was controlled to be 10 μM. The absorption spectra of retinoic acid / hydromagnesium composite powder in different polar solvents were tested. Figure 6 The corresponding quantitative results are shown in Table 3. From the test results, it can be seen that the absorption spectrum peaks of retinoic acid / hydromagnesium composite powder in various polar solvents (except glycerol) are basically around 356nm, and the absorbance is relatively similar. However, in glycerol, its absorption spectrum peak red-shifts to 396.5nm, and the absorbance also drops to 0.49, indicating that retinoic acid / hydromagnesium composite powder is suitable for use in solvents of different polarities, and is not highly dependent on the polarity of the solvent. In contrast, it is significantly dependent on viscosity, especially in high-viscosity solutions, where its absorption spectrum changes significantly.

[0086] Table 3 Absorption spectrum peak and absorbance of retinoic acid / hydromagnesium composite powder

[0087]

[0088] (3) Photostability test of retinoic acid / hydromagnesium composite powder in high viscosity solution:

[0089] The retinoic acid / hydromagnesium composite powder prepared in Example 1 was dispersed in trichloroethane, and then added to a high viscosity solution (wherein the high viscosity solution was composed of 99% glycerol and 1% deionized water, and its viscosity value was 956.0 cP), and the mixed concentration of the retinoic acid / hydromagnesium composite powder was controlled to be 10 μmol / L. The composite powder was irradiated under an excitation light source of 365 nm for 60 min, and its photostability was tested. The results are as follows: Figure 7 As shown in the results, it can be seen that the retinoic acid / hydromagnesium composite powder can still release strong light signals under long-term irradiation, and its light stability is excellent, which is suitable for long-term existence in correction fluid and can exert its effectiveness.

[0090] (4) Application of retinoic acid / hydromagnesium composite powder in correction fluids of different viscosities:

[0091] Specifically, the retinoic acid / hydromagnesium composite powder prepared in Example 1 was dispersed in three different correction fluids (correction fluid 1, correction fluid 2, and correction fluid 3), wherein the mixed concentration of the retinoic acid / hydromagnesium composite powder was controlled to be 1 μmol / L, and the luminescence intensity was observed. The results are as follows: Figure 8 As shown. Figure 8 It can be seen that the viscosity of the three correction fluids is different, among which the viscosity of correction fluid 1 is 1.83cP, the viscosity of correction fluid 2 is 2.42cP, and the viscosity of correction fluid 3 is 3.60cP. When retinoic acid / hydromagnesium composite powder is added to the correction fluids, the optical signal intensity is significantly different, and the signal intensity increases with the increase of viscosity. The specific values ​​are shown in Table 4. The results show that retinoic acid / hydromagnesium composite powder can have a good response effect on correction fluids of different viscosities, that is, it shows a positive correlation with viscosity, and can perceive the change of viscosity through the strength of the optical signal. It can be seen that the composite powder can provide the possibility of visual observation of the preparation process and thinness and thickness of the correction fluid.

[0092] Table 4 Light signal intensity of retinoic acid / hydromagnesium composite powder in correction fluids of different viscosities

[0093] Correction fluid types Fluorescence intensity Viscosity Correction fluid 1 159.3 1.83 Correction Fluid 2 198.6 2.42 Correction Fluid 3 399.5 3.60

[0094] The invention combines a natural product, retinoic acid, with hydromagnesia widely existing in nature to prepare a retinoic acid / hydromagnesia composite powder, fully utilizes the rotatability of the large conjugated structure of retinoic acid to realize response imaging of the viscosity of the correction fluid micro-region, and utilizes the basic magnesium carbonate characteristics of hydromagnesia to achieve the effects of smoke suppression and flame retardancy. At the same time, retinoic acid can not only reduce the surface polarity of natural hydromagnesia, improve its compatibility in a polymer matrix and greatly reduce the oil absorption value of natural hydromagnesia, but also is a natural carbon-forming agent, which can form a synergistic effect with the internal natural hydromagnesia, and has a great advantage in improving the comprehensive performance of the composite powder; in addition, the whiteness value of natural hydromagnesia reaches 96.0, has good covering power, and can meet the correction effect of correction fluid; finally, the obtained retinoic acid / hydromagnesia composite powder is prepared by a one-step method, the main raw materials are all from nature, belong to typical natural products, are very environmentally friendly, suitable for large-scale preparation and application, can not only increase the value of traditional natural stone mines, but also realize the mutual combination of multiple natural products to jointly improve the comprehensive performance of inorganic powders.

[0095] As can be seen from the above embodiments, the present invention provides a retinoic acid / hydromagnesium composite powder and its preparation method and application. The retinoic acid / hydromagnesium composite powder of the present invention is composed of retinoic acid and hydromagnesium, wherein retinoic acid is the outer shell of the composite powder, and hydromagnesium is the core of the composite powder, wherein the molar ratio of retinoic acid to hydromagnesium is 1 to 50:1. The retinoic acid / hydromagnesium composite powder of the present invention is prepared by mixing a hydromagnesium solution and a dehydrating agent dispersion with a retinoic acid solution in sequence, and then performing a dehydration condensation reaction. The retinoic acid / hydromagnesium composite powder of the present invention has a layer of retinoic acid on its surface, has a flexible conjugated structure, can release a weak light signal in a low-viscosity correction fluid, and releases a strong light signal in a high-viscosity correction fluid, which is helpful for the formulation design of the correction fluid. And the conjugated structure of retinoic acid makes it very easy to form carbon during the combustion process, and has a good synergistic flame retardant effect with the internal hydromagnesium.

[0096] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. Application of a retinoic acid / hydromagnesium composite powder in detecting the viscosity of correction fluid micro-areas, It is characterized in that Just mix the retinoic acid / hydromagnesium composite powder and correction fluid; The retinoic acid / hydromagnesium composite powder is composed of retinoic acid and hydromagnesium, wherein the retinoic acid is the outer shell of the composite powder and the hydromagnesium is the inner core of the composite powder; the molar ratio of the retinoic acid to the hydromagnesium is 100:4; The preparation method of the retinoic acid / hydromagnesium composite powder comprises the following steps: mixing a hydromagnesium solution and a dehydrating agent dispersion with a retinoic acid solution in sequence, and then performing a dehydration condensation reaction to obtain the retinoic acid / hydromagnesium composite powder; The D50 of the retinoic acid / hydromagnesium composite powder is 0.9 to 3.0 μm, wherein the D50 of the inner core is 0.8 to 2.8 μm; The mixing concentration of the retinoic acid / hydromagnesium composite powder is 1 μmol / L.

2. Use of the retinoic acid / hydromagnesium composite powder according to claim 1 in detecting the viscosity of correction fluid micro-areas, It is characterized in that The retinoic acid solution is formed by mixing retinoic acid and a solvent; the hydromagnesium solution is formed by mixing hydromagnesium and a solvent; the dehydrating agent dispersion is formed by mixing a dehydrating agent and a solvent; and the solvent is independently N,N-dimethylformamide.

3. Use of the retinoic acid / hydromagnesium composite powder according to claim 2 in detecting the viscosity of correction fluid micro-areas, It is characterized in that The dehydrating agent is K 2 CO 3 ; The molar ratio of the dehydrating agent to hydromagnesite is 100:

4.

4. Use of a retinoic acid / hydromagnesium composite powder according to claim 1 or 2 in detecting the viscosity of correction fluid micro-areas, It is characterized in that The temperature of the dehydration condensation reaction is 60° C., and the time of the dehydration condensation reaction is 24 hours.

5. Use of the retinoic acid / hydromagnesium composite powder according to claim 4 in detecting the viscosity of correction fluid micro-areas, It is characterized in that The product of the dehydration condensation reaction is sequentially filtered, precipitated, centrifuged, washed and freeze-dried; the freeze-drying temperature is -45°C and the freeze-drying time is 32 hours.