Solvent-free amphiphobic antibacterial ink and preparation method thereof

Through the homemade low-surface energy photosensitive resin and antibacterial filler of solvent-free double-substantial antibacterial ink, combined with micro-nano silica, the failure problem of UV antibacterial ink under high humidity and oil pollution is solved, and excellent waterproofing and oil resistance are achieved. Antibacterial properties extend coating life and reduce costs.

CN119081470AActive Publication Date: 2024-12-06TIANJIN UNIV
View PDF 7 Cites 0 Cited by

Patent Information

Application Number
CN202411275478.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-12
Publication Date
2024-12-06
Estimated Expiration
2044-09-12

AI Technical Summary

Technical Problem

Existing UV antibacterial inks are prone to failure under high humidity environment and oil pollution. The photosensitive reaction of conventional antibacterial agents causes discoloration and their performance decreases, making it difficult to maintain effectiveness in long-term use.

Method used

Solvent-free double-subic antibacterial ink is used to improve the waterproof and oil-resistant properties and antibacterial properties of the coating and extend the service life by making low-surface energy photosensitive resin and antibacterial filler.

Benefits of technology

It significantly improves the waterproof and oil resistance and antibacterial rate of the ink, reduces the adhesion of water and organic solvents, avoids the discoloration problem of antibacterial agents, extends the life of the coating, and reduces production costs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081470A_ABST
    Figure CN119081470A_ABST
Patent Text Reader

Abstract

According to the solvent-free type amphiphobic antibacterial ink and the preparation method thereof, through the synergistic effect of self-made low-surface-energy photosensitive resin, micro-nano silicon dioxide and self-made antibacterial filler, an ink film has excellent waterproof and oil-proof performance and self-cleaning performance, adhesion of water, organic solvents and the like to the surface of a coating can be greatly reduced, and the antibacterial performance of the coating is improved. Meanwhile, the antibacterial rate is excellent, and finally the problem that an existing packaging coating based on UV antibacterial ink is prone to failure in long-term use is effectively solved; besides, preparation raw materials are simple, reaction conditions are mild, fluorine-containing surfactants or long-carbon-chain silane coupling agents which are high in price and high in toxicity are not used, the production cost is low, large-scale production is facilitated, and the method can be applied to the technical field of packaging and can also be applied to the field of metal protection and glass protection surfaces.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the technical field of UV ink, and in particular to a UV-curable antibacterial ink. Background Art

[0002] In recent years, metal container packaging has turned to environmental friendliness, functionality, fast curing speed and high efficiency. Inks are mainly used in metal container packaging. Research on environmentally friendly inks is committed to developing solvent-free inks. Research on functional inks includes inks with antibacterial, waterproof and oil-proof properties to meet the needs of specific performance in the fields of electronics, optics and sensors. UV curing inks do not contain volatile organic compounds, have fast curing speed, low energy consumption and high efficiency, and have broad prospects.

[0003] There are four types of conventional antibacterial inks, namely antibacterial UV inks, antibacterial water-based inks, antibacterial water-based UV inks, and antibacterial alcohol inks. However, these four types of antibacterial inks have poor stability, are only feasible in the short term, and lack long-term effectiveness, especially in high humidity environments and when contaminated by oily pollutants, which greatly shortens their service life. In addition, conventional antibacterial agents such as quaternary ammonium salts, TiO2, nano-Ag, and ZnO have strong photosensitive reactions and are very easy to change color when exposed to light or stored for a long time. In addition, the performance of the antibacterial materials prepared by direct addition is significantly reduced. When exposed to water, Ag + It is easy to precipitate, resulting in a short antibacterial effectiveness period. Organic antibacterial agents such as quaternary ammonium salts will cause secondary pollution and other side effects, which makes it difficult to have application value in UV curing systems. Summary of the invention

[0004] In view of this, the present disclosure provides a solvent-free dual-repellent antibacterial ink and a preparation method thereof, which solves the problems that the current packaging coating based on UV antibacterial ink is easy to fail in long-term use and the conventional antibacterial agent used has a photosensitivity reaction causing discoloration.

[0005] To achieve the above-mentioned purpose of the invention, in the first aspect, the solvent-free dual-repellent antibacterial ink disclosed in the present invention comprises the following raw materials in parts by mass:

[0006] 2-25 parts of acrylic resin, 5-40 parts of epoxy resin, 5-25 parts of diluent, 1-15 parts of low surface energy photosensitive resin, 3-4 parts of fluorine-containing additives, 5-15 parts of micro-nano silica, 0.5-5 parts of antibacterial filler, 0.5-5.0 parts of defoaming agent, 0.5-5.0 parts of wetting and dispersing agent, 0.1-5.0 parts of leveling agent, and 0.5-10 parts of photoinitiator.

[0007] In the present disclosure and possible embodiments, the method for preparing the low surface energy photosensitive resin includes:

[0008] After free radical copolymerization of a sulfhydryl chain transfer agent, a fluoro-containing monomer of p-methacrylic acid and poly(ethylene glycol) methyl ether acrylate, glycidyl methacrylate is added to the copolymerization product to introduce a photosensitive group at the tail end of the sulfhydryl chain transfer agent to obtain the low surface energy photosensitive resin.

[0009] In the present disclosure and possible embodiments, the synthesis route of the low surface energy photosensitive resin is:

[0010]

[0011] In the present disclosure and possible embodiments, the method for preparing the antibacterial filler comprises:

[0012] 5-10 parts of nano zinc oxide are dispersed in 90 parts of anhydrous ethanol, 1-2 parts of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride are added, 1-2 parts of dopamine are self-assembled on the surface of the nano zinc oxide to form a polydopamine functional interface, and then a cerium nitrate solution is added to perform an in-situ reduction reaction; after the in-situ reduction reaction is completed, the system is placed in a 0.2MPa, 100°C, N2 autoclave, 10-20 parts of calcined flaky micron particles are added, and the reaction is carried out for 12 hours to obtain the antibacterial filler.

[0013] In the present disclosure and possible embodiments, the flaky micron particles are selected from a mixture of one or more of boron nitride, talc, hydrotalcite, montmorillonite, mica powder and kaolin, and have a particle size D≤300 mesh.

[0014] In the present disclosure and possible embodiments, the micro-nano silicon dioxide is a composite of micron SiO2 and nano SiO2, the particle size range of the micron SiO2 is 5-20um, the particle size range of the nano SiO2 is 7-50nm, and the mass ratio of the micron SiO2 to the nano SiO2 is 7-9:1-3.

[0015] In the present disclosure and possible embodiments, the acrylic resin is a mixture of one or more of acrylic polyurethane resin, pure acrylic resin and acrylic epoxy resin; the epoxy resin is a UV-curable difunctional epoxy resin; and the diluent is an acrylic monomer and an epoxy monomer.

[0016] In the present disclosure and possible embodiments, the epoxy resin is a UV-curable difunctional epoxy resin which is a mixture of one or more of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester, bis((3,4-epoxycyclohexyl)methyl)adipate and (3,4,3',4'-diepoxy)dicyclohexane.

[0017] In the present disclosure and possible embodiments, the acrylic monomer is one or more of trimethylolpropane triacrylate, tripropylene glycol diacrylate and 1,6-hexanediol diacrylate;

[0018] The epoxy monomer is a mixture of one or more of pentaerythritol glycidyl ether, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether and 3-ethyl-3-hydroxymethyloxetane.

[0019] In a second aspect, a method for preparing the solvent-free dual-repellent antibacterial ink according to any one of the first aspects comprises:

[0020] After all the liquid raw materials are mixed and dispersed for 10-30 minutes, all the solid raw materials except the antibacterial filler are added to the liquid raw material mixture and continue to disperse and stir for 30-50 minutes; finally, the antibacterial filler is added and stirred and dispersed for 10-20 minutes. After the dispersion is completed, it is placed in a black container away from light to obtain the solvent-free dual-repellent antibacterial ink; the particle size D of the ink is controlled to be ≤10um, and the viscosity is 100-800cps.

[0021] The present invention has the beneficial effects:

[0022] The solvent-free dual-repellent antibacterial ink disclosed in the present invention, through the self-made new type of low surface photosensitive resin, makes the ink film have better water and oil resistance and self-cleaning properties than commercially available low surface energy resins, can greatly reduce the adhesion of water and organic solvents on the coating surface, so as to further prevent the breeding of bacteria, and finally effectively solve the problem that the current packaging coating based on UV antibacterial ink is easy to fail in long-term use; and the self-made antibacterial filler, because it does not use traditional antibacterial agents that are easy to change color and has been modified, is not only not easy to change color, but also has excellent antibacterial rate; through the use of micro-nano silica, on the one hand, it provides a dual-repellent nano-microstructure, and on the other hand, it improves the wear resistance and hardness of the coating, which assists At the same time, it extends the life of the coating; therefore, the present invention utilizes the synergistic effect of a homemade low surface energy photosensitive resin, a homemade antibacterial filler and nano-silica, so that the ink of this patent has multiple properties that are significantly outstanding compared to conventional antibacterial UV inks; in addition, the preparation raw materials are simple, the reaction conditions are mild, and no expensive and highly toxic fluorinated surfactants or long-chain silane coupling agents are used, the production cost is reduced, the color change problem of the raw materials caused by the antibacterial agent is avoided, and it is easy to scale up the production; moreover, the ink of the present invention can be used not only in the field of packaging technology, but also in the field of metal protection and glass protection surfaces, and through its effective antibacterial and dirt adhesion reduction properties, efficient energy utilization is achieved. BRIEF DESCRIPTION OF THE DRAWINGS

[0023] The above and other objects, features and advantages of the present disclosure will become more apparent through the following description of the embodiments of the present disclosure with reference to the accompanying drawings, in which:

[0024] Figure 1-1 It is the test trace effect of the ink highlighter pen of the embodiments 1-5 of the present disclosure and the comparative example;

[0025] Figure 1-2 This is the effect of the ink of Examples 1-5 of the present disclosure and the comparative example after wiping off the traces of the fluorescent pen test;

[0026] Figure 2 These are the antibacterial test results of inks of Examples 1-5 and the comparative example of the present disclosure. DETAILED DESCRIPTION

[0027] The present disclosure is described below based on specific embodiments, but it is worth noting that the present disclosure is not limited to these specific embodiments. In the detailed description of the present disclosure below, some specific details are described in detail. However, for the parts that are not described in detail, those skilled in the art can also fully understand the present disclosure.

[0028] At the same time, unless the context clearly requires otherwise, the words "include", "comprises" and similar words throughout the specification and claims should be interpreted as inclusive rather than exclusive or exhaustive; that is, the meaning is "including but not limited to".

[0029] Unless otherwise specified, the raw materials or reagents used in the embodiments of the present disclosure can be purchased or synthesized using conventional methods with reference to relevant literature.

[0030] In each embodiment of the present disclosure, the method for preparing the solvent-free dual-repellent antibacterial ink comprises the following steps:

[0031] 1. Preparation of low surface energy photosensitive resin:

[0032] At 75°C, using azobisisobutyl cyanide (AIBN) initiator, a sulfur-based chain transfer agent (CTA), a fluoromonomer containing p-methacrylic acid, and poly(ethylene glycol) methyl ether acrylate undergo free radical copolymerization, and glycidyl methacrylate is added to the copolymerization product in order to introduce a photosensitive group at the end of CTA, and finally obtain a hydrophobic and oleophobic photosensitive resin with low surface energy. The specific synthesis route is:

[0033]

[0034] 2. Preparation of micro-nano silicon dioxide:

[0035] Micron-sized SiO2 and nano-sized SiO2 are compounded in a mass ratio of 7-9:1-3 to obtain micro-nano silicon dioxide; wherein the particle size range of the micron-sized SiO2 is 5-20um, and the particle size range of the nano-sized SiO2 is 7-50nm.

[0036] 3. Preparation of antibacterial fillers:

[0037] 5-10 parts of nano zinc oxide are dispersed in 90 parts of anhydrous ethanol, 1-2 parts of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride are added, 1-2 parts of dopamine are used to self-assemble on the surface of the nano zinc oxide to form a PDA (polydopamine) functional interface, and then in a closed environment at 80°C, cerium nitrate solution (mass concentration is 0.2%) is added for in-situ reduction reaction, and CeO2 is further adsorbed by reacting with 5-10 parts of cerium nitrate through the PDA functional port; then the system is transferred to a 0.2MPa, 100°C, N2 autoclave, 10-20 parts of calcined flaky microparticles are added, and a hydrothermal reaction is carried out for 12 hours to obtain an antibacterial filler.

[0038] In a specific embodiment, the calcined flaky micron particles are selected from a mixture of one or more of boron nitride, talc, hydrotalcite, montmorillonite, mica powder and kaolin, and the particle size D is ≤300 mesh.

[0039] 4. Preparation of solvent-free dual-repellent antibacterial ink:

[0040] (1) By weight, the raw material composition of the solvent-free dual-repellent antibacterial ink is:

[0041] Acrylic resin 2-25%, epoxy resin 5-40%, diluent 5-25%, low surface energy photosensitive resin 1-15%, fluorine-containing additive 3-4 parts, micro-nano silica 5-15%, antibacterial filler 0.5-5%, defoamer 0.5-5.0%, wetting dispersant 0.5-5.0%, leveling agent 0.1-5.0%, photoinitiator 0.5-10%.

[0042] In a specific embodiment, the acrylic resin is a mixture of one or more of polyurethane acrylate resin (Agisyn 248), pure acrylic resin (Agisyn 262) and acrylic epoxy resin (Lancolu, L-6111).

[0043] In a specific embodiment, the epoxy resin is a UV-curable difunctional epoxy resin, specifically a mixture of one or more of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester, bis((3,4-epoxycyclohexyl)methyl)adipate, and (3,4,3',4'-diepoxy)dicyclohexane.

[0044] In a specific embodiment, the diluent is an acrylic monomer and an epoxy monomer. The acrylic monomer is one or more of trimethylolpropane triacrylate (TMPTA), tripropylene glycol diacrylate (TPGDA), and 1,6-hexanediol diacrylate (HDDA). The epoxy monomer is a mixture of one or more of pentaerythritol glycidyl ether, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether, and 3-ethyl-3-hydroxymethyloxetane.

[0045] In a specific embodiment, the fluorine-containing additive is DSP-859F from Zhongshan Jieshida Fine Chemicals; SiO2 with micron and nanoparticle sizes is purchased from Pioneer Nanomaterials (20nm:5um=9:2); the defoaming agent is BYKJET-9151; the wetting and dispersing agent is BYKJET-9151; the leveling agent is BYK-UV3510; and the photoinitiator is IGM from BASF of Germany.

[0046] (2) After all the liquid raw materials in the raw material composition are placed in a stirring tank and stirred and dispersed for 10-30 minutes, all the solid raw materials except the antibacterial filler are added to the above liquid and dispersed and stirred for 30-50 minutes; finally, the antibacterial filler is added and dispersed for 10-20 minutes. After the dispersion is completed, the solid raw materials are placed in a black barrel in a dark place to obtain a solvent-free dual-repellent antibacterial ink with a particle size D≤10um and a viscosity of 100-800cps.

[0047] The following are specific embodiments of the present disclosure.

[0048] Example 1

[0049] 1. Preparation of low surface energy photosensitive resin:

[0050] 0.1 parts of CAT and 50 parts of butyl acetate were added to the reactor, and a mixture of 10 parts of methacrylate heptadecafluorodecyl and 0.01 parts of AIBN was added dropwise at 75°C. After the reaction for 1.5 hours, 10 parts of poly(ethylene glycol) methyl ether acrylate (z=19) were added, and the reaction was continued for 4 hours. After the reaction was completed, 2 drops of triethylamine were added, the temperature was raised to 80°C, and 0.1 parts of glycidyl methacrylate were added dropwise until the carboxyl absorption peak of infrared detection disappeared; after the reaction was completed, the solvent was removed by rotary evaporation and the viscous liquid was collected to finally obtain a low surface energy photosensitive resin.

[0051] 2. Preparation of antibacterial fillers:

[0052] Disperse 5 parts of nano zinc oxide in 90 parts of anhydrous ethanol, add 1 part of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride and stir to react at 50°C for 4 hours, add 1 part of dopamine to self-assemble in the above solution to form a PDA functional interface, then add 5 parts of cerium nitrate solution with a mass concentration of 2% in a closed environment at 80°C for in-situ reduction reaction, then transfer the system to a 0.2MPa, 100°C, N2 autoclave, add 10 parts of calcined boron nitride, react for 12 hours to obtain an antibacterial filler.

[0053] 3. Preparation of solvent-free dual-repellent antibacterial ink:

[0054] (1) Ink raw material composition:

[0055] 15 parts of difunctional acrylic polyurethane resin, 30 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester, 5 parts of TPGDA, 16 parts of 3-ethyl-3-hydroxymethyloxetane, 10 parts of low surface energy photosensitive resin, 3 parts of fluorine-containing additives, 7.5 parts of micro-nano silica, 3 parts of antibacterial filler, 0.5 parts of defoaming agent, 2 parts of wetting and dispersing agent, 0.1 parts of leveling agent, and 7.9 parts of photoinitiator.

[0056] (2) Preparation process:

[0057] After all the liquids were placed in a stirring tank and stirred and dispersed for 15 minutes, all solids except the antibacterial filler were added and continued to be dispersed and stirred for 35 minutes. Finally, the antibacterial filler was added and stirred and dispersed for 20 minutes. After the dispersion was completed, it was placed in a black container away from light to obtain the solvent-free dual-repellent antibacterial ink of this embodiment 1.

[0058] Example 2

[0059] 1. Preparation of low surface energy photosensitive resin:

[0060] Take 0.2 parts of CAT and 50 parts of butyl acetate and add them to the reactor. Add 15 parts of methacrylate heptafluorodecyl ester and 0.015 parts of AIBN dropwise at 75°C. After reacting for 1.5 hours, add 10 parts of ethylene glycol methyl ether acrylate (z=17) and continue to react for 4 hours. After the reaction is completed, add 2 drops of triethylamine, raise the temperature to 80°C, and add 0.2 parts of glycidyl methacrylate dropwise until the infrared detection carboxyl absorption peak disappears; after the reaction is completed, remove the solvent by rotary evaporation and collect the viscous liquid, and finally obtain a hydrophobic and oleophobic low surface energy photosensitive resin.

[0061] 2. Preparation of antibacterial fillers:

[0062] Disperse 5 parts of nano zinc oxide in 90 parts of anhydrous ethanol, add 1.5 parts of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride and stir to react at 50°C for 4 hours, add 2 parts of dopamine to self-assemble in the above solution to form a PDA functional interface, then add 5 parts of cerium nitrate solution with a mass concentration of 2% in a closed environment at 80°C for in-situ reduction reaction, then transfer it to a 0.2MPa, 100°C, N2 autoclave, add 10 parts of calcined hydrotalcite, react for 12 hours to obtain an antibacterial filler.

[0063] 3. Preparation of solvent-free dual-repellent antibacterial ink:

[0064] (1) Ink raw material composition:

[0065] 25 parts of pure acrylic resin and acrylic epoxy resin, 10 parts of bis((3,4-epoxycyclohexyl)methyl)adipate, 10 parts of TPGDA and pentaerythritol glycidyl ether (1:1), 3 parts of fluorine-containing additives, 15 parts of low surface photosensitivity resin, 10 parts of micro-nano silica, 2 parts of antibacterial filler, 5 parts of defoamer, 5 parts of wetting and dispersing agent, 5 parts of leveling agent, and 10 parts of photoinitiator.

[0066] (2) Preparation process:

[0067] After all the liquids were placed in a stirring tank and stirred and dispersed for 15 minutes, all solids except the antibacterial filler were added and continued to be dispersed and stirred for 50 minutes. Finally, the antibacterial filler was added and stirred and dispersed for 10 minutes. After the dispersion was completed, it was placed in a black container away from light to obtain the solvent-free dual-repellent antibacterial ink of this embodiment 2.

[0068] Example 3

[0069] 1. Preparation of low surface energy photosensitive resin:

[0070] Take 0.2 parts of CAT and 50 parts of butyl acetate and add them to the reactor. Add 10 parts of methacrylate heptadecafluorodecyl and 0.01 parts of AIBN dropwise at 75°C. After 1.5 hours of reaction, add 15 parts of ethylene glycol methyl ether acrylate (z=19) and continue to react for 4 hours. After the reaction is completed, add 2 drops of triethylamine, raise the temperature to 80°C, and add 0.2 parts of glycidyl methacrylate until the infrared detection carboxyl absorption peak disappears. After the reaction is completed, remove the solvent by rotary evaporation and collect the viscous liquid to finally obtain a hydrophobic and oleophobic low surface energy photosensitive resin.

[0071] 2. Preparation of antibacterial fillers:

[0072] 7 parts of nano zinc oxide were dispersed in 90 parts of anhydrous ethanol, 2 parts of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride were added and stirred at 50°C for 4 hours, 2 parts of dopamine were added to the above solution to self-assemble to form a PDA functional interface, and then 10 parts of cerium nitrate solution with a mass concentration of 2% were added in a closed environment at 80°C for in-situ reduction reaction, and then it was transferred to a 0.2MPa, 100°C, N2 autoclave, 14 parts of calcined talc were added, and the reaction was carried out for 12 hours to obtain an antibacterial filler.

[0073] 3. Preparation of solvent-free dual-repellent antibacterial ink:

[0074] (1) Ink raw material composition:

[0075] 5 parts of acrylic polyurethane resin and pure acrylic resin, 40 parts of bis((3,4-epoxycyclohexyl)methyl)adipate and (3,4,3',4'-diepoxy)dicyclohexane film-forming agent, 10 parts of HDDA, 15 parts of neopentyl glycol diglycidyl ether, 4 parts of fluorine-containing additives, 5 parts of low surface photosensitivity resin, 10 parts of micro-nano silica, 0.5 parts of antibacterial filler, 1.0 parts of defoamer, 1.0 parts of wetting and dispersing agent, 0.5 parts of leveling agent, and 8 parts of photoinitiator.

[0076] (2) Preparation process:

[0077] After all the liquids were placed in a stirring tank and stirred and dispersed for 20 minutes, all solids except the antibacterial filler were added and continued to be dispersed and stirred for 50 minutes. Finally, the antibacterial filler was added and stirred and dispersed for 10 minutes. After the dispersion was completed, it was placed in a black container away from light to obtain the solvent-free dual-repellent antibacterial ink of Example 3.

[0078] Example 4

[0079] 1. Preparation of low surface energy photosensitive resin:

[0080] Take 0.15 parts of CAT and 50 parts of butyl acetate and add them to the reactor. Add 10 parts of methacrylate heptafluorodecyl ester and 0.01 parts of AIBN dropwise at 75°C. After reacting for 1.5 hours, continue to add 20 parts of ethylene glycol methyl ether acrylate (z=17) and continue to react for 4 hours. After the reaction is completed, add 2 drops of triethylamine, increase the temperature to 80°C, and add 0.15 parts of glycidyl methacrylate until the infrared detection carboxyl absorption peak disappears; after the reaction is completed, remove the solvent by rotary evaporation and collect the viscous liquid, and finally obtain a hydrophobic and oleophobic low surface energy photosensitive resin.

[0081] 2. Preparation of antibacterial fillers:

[0082] Disperse 5 parts of nano zinc oxide in 90 parts of anhydrous ethanol, add 1 part of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride and stir to react at 50°C for 4 hours, add 1.5 parts of dopamine to self-assemble in the above solution to form a PDA functional interface, then add 10 parts of cerium nitrate solution with a mass concentration of 2% in a closed environment at 80°C for in-situ reduction reaction, then transfer it to a 0.2MPa, 100°C, N2 autoclave, add 10 parts of calcined mica powder, react for 12 hours to obtain an antibacterial filler.

[0083] 3. Preparation of solvent-free dual-repellent antibacterial ink:

[0084] (1) Ink raw material composition:

[0085] 5 parts of pure acrylic resin, 10 parts of acrylic polyurethane resin, 30 parts of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester, 5 parts of TMPTA, 20 parts of 3-ethyl-3-hydroxymethyloxetane, 4 parts of fluorine-containing additives, 9 parts of low surface photosensitivity resin, 11.5 parts of micro-nano silica, 5 parts of antibacterial filler, 2 parts of defoamer, 2 parts of wetting and dispersing agent, 0.5 parts of leveling agent, and 7 parts of photoinitiator.

[0086] (2) Preparation process:

[0087] After all the liquids were placed in a stirring tank and stirred and dispersed for 10 minutes, all solids except the antibacterial filler were added and continued to be dispersed and stirred for 50 minutes. Finally, the antibacterial filler was added and stirred and dispersed for 20 minutes. After the dispersion was completed, it was placed in a black container away from light to obtain the solvent-free dual-repellent antibacterial ink of Example 4.

[0088] Example 5

[0089] 1. Preparation of low surface energy photosensitive resin:

[0090] Take 0.2 parts of CAT and 50 parts of butyl acetate and add them to the reactor. Add 15 parts of methacrylate heptafluorodecyl ester and 0.01 parts of AIBN dropwise at 75°C. After reacting for 1.5 hours, continue to add 15 parts of ethylene glycol methyl ether acrylate (z=19) and continue to react for 4 hours. After the reaction is completed, add 2 drops of triethylamine, increase the temperature to 80°C, and add 0.2 parts of glycidyl methacrylate until the infrared detection carboxyl absorption peak disappears; after the reaction is completed, remove the solvent by rotary evaporation and collect the viscous liquid, and finally obtain a hydrophobic and oleophobic low surface energy photosensitive resin.

[0091] 2. Preparation of antibacterial fillers:

[0092] Disperse 10 parts of nano zinc oxide in 90 parts of anhydrous ethanol, add 1 part of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride and stir to react at 50°C for 4 hours, add 2 parts of dopamine to self-assemble in the above solution to form a PDA functional interface, then add 10 parts of cerium nitrate solution with a mass concentration of 2% in a closed environment at 80°C for in-situ reduction reaction, then transfer it to a 0.2MPa, 100°C, N2 autoclave, add 20 parts of calcined kaolin, react for 12 hours to obtain an antibacterial filler.

[0093] 3. Preparation of solvent-free dual-repellent antibacterial ink:

[0094] (1) Ink raw material composition:

[0095] 15 parts of acrylic epoxy resin, 25 parts of (3,4,3',4'-diepoxy)bicyclohexane, 5 parts of TMPTA, 5 parts of TPGDA, 15 parts of 3-ethyl-3-hydroxymethyloxetane, 12 parts of low surface photosensitivity resin, 3 parts of fluorine-containing additives, 2 parts of antibacterial fillers, 8.5 parts of micro-nano silica, 1.0 parts of defoaming agent, 1.0 parts of wetting and dispersing agent, 0.5 parts of leveling agent, and 7 parts of photoinitiator.

[0096] (2) Preparation process:

[0097] After all the liquids were placed in a stirring tank and stirred and dispersed for 15 minutes, all solids except the antibacterial filler were added and continued to be dispersed and stirred for 30 minutes. Finally, the antibacterial filler was added and stirred and dispersed for 20 minutes. After the dispersion was completed, it was placed in a black container away from light to obtain the solvent-free dual-repellent antibacterial ink of Example 5.

[0098] Performance Test:

[0099] In order to compare and illustrate the ink performance of Examples 1-5, UV flexographic varnish UV-5100 produced by Zhongshan Kairui High-tech Application Materials Co., Ltd. was selected as a comparative example.

[0100] 1. The ink properties and properties after coating of the embodiments and comparative examples were measured. The results are shown in Table 1:

[0101] Table 1: Performance of inks after coating in the examples and comparative examples

[0102] Viscosity cPs / 25℃ odor Appearance Glossiness Touch Resistant tape Highlighter resistant Example 1 459 No obvious smell Light yellow opaque 20 Curing Curing Curing Example 2 399 No obvious smell Milky white opaque 17 Curing Curing Curing Example 3 389 No obvious smell White opaque 19 Curing Curing Curing Example 4 425 No obvious smell White opaque 22 Curing Curing Curing Example 5 401 No obvious smell White opaque 18 Curing Curing Curing Comparative Example 125 Resin smell transparent 94 Curing Curing Curing

[0103] It can be seen from Table 1 that in Examples 1-5, the main cross-linked resin is an epoxy UV resin, which reduces the odor of varnish and avoids the odor of acrylic resin-based ink. In the comparative example, no relevant micro-nanoparticles are added, and the coating shows transparency, but has a resin odor.

[0104] 2. Determination of contact angle:

[0105] Referring to GB / T 30447-2013 "Nanofilm Contact Angle Measurement Method", the instrument used was Shanghai Zhongchen JC2000D1 dynamic contact angle measuring instrument. Each sample was scraped with a 5μm offset applicator, each droplet was 5μl, the sliding angle was 30ul, and 3 parallel experiments were set. The experimental results are shown in Tables 2 and 3:

[0106] Table 2 Comparison of contact angles between the low surface energy photosensitive resin in the embodiment and the commercially available low surface energy resin

[0107]

[0108]

[0109] It can be seen from the data in Table 2 that the low surface energy photosensitive resins of Examples 1-5 have significantly improved amphiphobic properties compared to commercially available low surface energy resins.

[0110] Table 3 Contact angle test of ink of example and comparative example

[0111] Water contact angle WCA Oil contact angle OCA Slip Angle WSA Example 1 106-110 88-91 30-35 Example 2 108-112 86-89 33-37 Example 3 107-113 89-92 35-40 Example 4 109-112 87-90 38-42 Example 5 110-114 89-94 20-35 Comparative Example 45-50 30-45 /

[0112] Note: The water is deionized water and rapeseed oil is used for oil contact angle test.

[0113] It can be seen from the data in Table 2 that the samples of Examples 1-5 have excellent hydrophobicity and oleophobicity, namely WCA>90°, OCA>90°, and SA<60°, which are significantly better than the samples of the comparative example.

[0114] The solvent-free antibacterial ink film of the present invention has excellent water contact angle and oil contact angle, which cannot be achieved by the products currently on the market. The good waterproof and oil-proof and self-cleaning properties can greatly reduce the adhesion of water and organic solvents on the coating surface, thereby further preventing the growth of bacteria, and effectively solving the problem that the current packaging coating based on UV antibacterial ink is prone to failure during long-term use.

[0115] 3. Fluorescent pen resistance test:

[0116] When conducting a fluorescent pen resistance test, after the fluorescent pen is applied, the oily fluorescent ink on the surface of the coating gradually shrinks into small droplets. The smaller the droplets, the more obvious the effect. That is, gently wipe off the ink on the surface. The fewer the remaining traces, the better the effect.

[0117] Depend on Figure 1-1 , 1-2 It can be seen from the test results that the fluorescent pen marks of the comparative example were not erased; the fluorescent pen marks of Examples 1-5 could all be erased. In addition, after being applied with the fluorescent pen, the coating surface shrank to a certain extent and shrunk into a small droplet state.

[0118] 4. Antibacterial test:

[0119] Test basis: JIS Z 2801:2012 "Testing and evaluation of antibacterial properties of antibacterial products"; Test bacteria: Escherichia coli ATCC 8739; Staphylococcus aureus ATCC 6538p; Test samples are 6 pieces per group, and the test sample size is 4*4cm; Test results are shown in Table 3.1-Table 3.7 and Figure 2 :

[0120] Table 3.1 Blank Example

[0121]

[0122] Table 3.2 Antibacterial test results of Example 1

[0123]

[0124] Table 3.3 Antibacterial test results of Example 2

[0125]

[0126]

[0127] Table 3.4 Antibacterial test results of Example 3

[0128]

[0129] Table 3.5 Antibacterial test results of Example 4

[0130]

[0131]

[0132] Table 3.6 Antibacterial test results of Example 5

[0133]

[0134] Table 3.7 Comparative Example Antibacterial Test Results

[0135]

[0136]

[0137] It can be seen from the data in the above tables that the antibacterial rates of the inks of Examples 1-5 against Escherichia coli and Staphylococcus aureus are all above 95%, while the comparative example is not antibacterial.

[0138] Figure 2The antibacterial test graph shows that after 24 hours, Escherichia coli and Staphylococcus aureus multiplied very densely in the blank control, and the same was true for the comparative example, while no obvious colonies appeared in Examples 1-5, indicating that the inks of Examples 1-5 have better antibacterial properties.

[0139] The following conclusions can be drawn from the performance tests of the above comparative examples and embodiments:

[0140] The solvent-free antibacterial ink of the present invention has good antibacterial property, waterproof and oil-proof effect and anti-ink adhesion performance, and its comprehensive performance cannot be achieved by the products on the market, filling the gap of high hydrophobicity and oleophobicity of UV antibacterial waterproof and oil-proof coating in the current market; the solvent-free antibacterial waterproof and oil-proof ink can be applied not only to the field of packaging technology, but also to the field of metal protection and glass protection surface, and realizes efficient utilization of energy through its effective antibacterial and dirt adhesion reduction performance.

[0141] The above-described embodiments are only embodiments of the present disclosure, and the descriptions thereof are relatively specific and detailed, but they cannot be construed as limiting the scope of the present disclosure. It should be noted that, for a person of ordinary skill in the art, without departing from the concept of the present disclosure, several variations, equivalent substitutions, improvements, etc. may be made, all of which fall within the scope of protection of the present disclosure. Therefore, the scope of protection of the present disclosure shall be subject to the attached claims.

Claims

1. A solvent-free dual-repellent antibacterial ink, characterized in that: The raw material composition is as follows by weight: 2-25 parts of acrylic resin, 5-40 parts of epoxy resin, 5-25 parts of diluent, 1-15 parts of low surface energy photosensitive resin, 3-4 parts of fluorine-containing additives, 5-15 parts of micro-nano silica, 0.5-5 parts of antibacterial filler, 0.5-5.0 parts of defoaming agent, 0.5-5.0 parts of wetting and dispersing agent, 0.1-5.0 parts of leveling agent, and 0.5-10 parts of photoinitiator.

2. The solvent-free dual-repellent antibacterial ink according to claim 1, characterized in that: The method for preparing the low surface energy photosensitive resin comprises: After free radical copolymerization of a sulfhydryl chain transfer agent, a fluoro-containing monomer of p-methacrylic acid and poly(ethylene glycol) methyl ether acrylate, glycidyl methacrylate is added to the copolymerization product to introduce a photosensitive group at the tail end of the sulfhydryl chain transfer agent to obtain the low surface energy photosensitive resin.

3. The solvent-free dual-repellent antibacterial ink according to claim 2, characterized in that: The synthesis route of the low surface energy photosensitive resin is: 。 4. The solvent-free dual-repellent antibacterial ink according to any one of claims 1 to 3, characterized in that: The preparation method of the antibacterial filler comprises: 5-10 parts of nano zinc oxide are dispersed in 90 parts of anhydrous ethanol, 1-2 parts of dimethyloctadecyl[3-(trimethoxysilyl)propyl]ammonium chloride are added, 1-2 parts of dopamine are self-assembled on the surface of the nano zinc oxide to form a polydopamine functional interface, and then a cerium nitrate solution is added to perform an in-situ reduction reaction; after the in-situ reduction reaction is completed, the system is placed in a 0.2 MPa, 100°C, N2 autoclave, 10-20 parts of calcined flaky micron particles are added, and the reaction is carried out for 12 hours to obtain the antibacterial filler.

5. The solvent-free dual-repellent antibacterial ink according to claim 4, characterized in that: The flaky micron particles are selected from a mixture of one or more of boron nitride, talc, hydrotalcite, montmorillonite, mica powder and kaolin, and have a particle size D≤300 meshes.

6. The solvent-free dual-repellent antibacterial ink according to any one of claims 1 to 3 or 5, characterized in that: The micro-nano silicon dioxide is a composite of micron SiO2 and nano SiO2, the particle size of the micron SiO2 is in the range of 5-20 um, the particle size of the nano SiO2 is in the range of 7-50 nm, and the mass ratio of the micron SiO2 to the nano SiO2 is 7-9:1-3.

7. The solvent-free dual-repellent antibacterial ink according to claim 6, characterized in that: The acrylic resin is a mixture of one or more of acrylic polyurethane resin, pure acrylic resin and acrylic epoxy resin; the epoxy resin is a UV-curable difunctional epoxy resin; and the diluent is an acrylic monomer and an epoxy monomer.

8. The solvent-free dual-repellent antibacterial ink according to claim 7, characterized in that: The epoxy resin is a UV-curable bifunctional epoxy resin which is a mixture of one or more of 3,4-epoxycyclohexylcarboxylic acid-3',4'-epoxycyclohexyl methyl ester, bis((3,4-epoxycyclohexyl)methyl)adipate and (3,4,3',4'-diepoxy)bicyclohexane.

9. The solvent-free dual-repellent antibacterial ink according to claim 7, characterized in that: The acrylic monomer is one or more of trimethylolpropane triacrylate, tripropylene glycol diacrylate and 1,6-hexanediol diacrylate; The epoxy monomer is a mixture of one or more of pentaerythritol glycidyl ether, 1,4-butanediol diglycidyl ether, neopentyl glycol diglycidyl ether and 3-ethyl-3-hydroxymethyloxetane.

10. A method for preparing the solvent-free dual-repellent antibacterial ink according to any one of claims 1 to 9, characterized in that: include: After all the liquid raw materials are mixed and dispersed for 10-30 minutes, all the solid raw materials except the antibacterial filler are added to the liquid raw material mixture and continue to disperse and stir for 30-50 minutes; finally, the antibacterial filler is added and stirred and dispersed for 10-20 minutes. After the dispersion is completed, it is placed in a black container away from light to obtain the solvent-free dual-repellent antibacterial ink; the particle size D of the ink is controlled to be ≤10um, and the viscosity is 100-800 cps.

Citation Information

Patent Citations

  • Preparation method for poly-dopamine modified ceramic particle nonwoven diaphragm

    CN105390642A

  • Amphiphobic layer and printing ink packaging film containing same

    CN107502165A

  • Durable antibacterial and antiviral super-amphiphobic coating and preparation method thereof

    CN114058223A

  • Resin emulsion including silicon compound, method of producing the same and resin composition for aqueous paint including the resin emulsion

    JP2002138123A

  • A-b block copolymer, method for producing a-b block copolymer, resin-treated pigment composition, method for producing resin-treated pigment composition, and use thereof