Water-based anti-corrosion finishing paint emulsion for offshore wind power blade and preparation method of water-based anti-corrosion finishing paint emulsion

By modifying the aqueous hybrid emulsion of hollow nanosilica combined with acrylate and phosphate monomers, the corrosion problem of offshore wind blades in extreme environments is solved, the hardness and wear resistance of the coating are improved, and the hardness and wear resistance of the coating are achieved. Environmentally friendly and efficient anti-corrosion effect.

CN119081495APending Publication Date: 2024-12-06ZHEJIANG SATELLITE PETRO CHEM CO LTD +1
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411432085.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-14
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Offshore wind blades are susceptible to surface corrosion caused by salt accumulation in extreme marine environments. The existing solvent-based anticorrosion emulsion coatings are prone to peel off when impacted by external forces, and cannot effectively resist corrosion. Environmental protection problems need to be solved.

Method used

Using silane-modified hollow nanosilica combined with acrylate and phosphate monomer as the topcoat, the coating hardness and wear resistance are improved and the substrate is enhanced by optimizing the material formulation and preparation process. Adhesion to resist the erosion of acid and alkali corrosive media.

Benefits of technology

It significantly improves the hardness and wear resistance of the coating, extends the service life, enhances the protection performance of a variety of corrosive media, and meets green and environmental protection requirements, avoids solvent contamination.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081495A_ABST
    Figure CN119081495A_ABST
Patent Text Reader

Abstract

The invention provides a water-based anticorrosive finishing paint emulsion for offshore wind power blades and a preparation method thereof, and relates to the technical field of preparation of water-based anticorrosive finishing paint emulsions. The water-based anticorrosive finishing paint emulsion is an inorganic-organic hybrid emulsion compounded by silane modified hollow nano silicon dioxide, an acrylate monomer and a phosphate monomer. The defects in the prior art are overcome, silane modified hollow nano silicon dioxide in the prepared inorganic-organic hybrid emulsion can remarkably improve the hardness and wear resistance of a coating, the acrylate monomer provides a stable basis for the coating due to the good film-forming property and weather resistance of the acrylate monomer, and due to introduction of the phosphate monomer, the wear resistance of the coating is greatly improved. And a chelating structure is formed with a metal base material, so that the adhesive force with the base material is enhanced, the coating can effectively resist corrosion of corrosive media such as acid and alkali, and the coating has excellent corrosion resistance.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of water-based anti-corrosion topcoat emulsion preparation, and in particular to a water-based anti-corrosion topcoat emulsion for offshore wind turbine blades and a preparation method thereof. Background Art

[0002] Wind energy, as an outstanding representative of renewable and clean energy, is gradually becoming the focus of global energy transformation, and governments around the world are competing to promote its rapid development. At present, the total installed capacity of offshore wind power in the world has jumped to more than 35GW, of which the new capacity in 2020 exceeded the 6GW mark. China leads the world with more than 3GW of new installed capacity, accounting for 50.45%, demonstrating its strong momentum in this field. However, the vigorous development of offshore wind power is not without challenges. Faced with extreme marine environments such as high temperature, high humidity and high salt spray, the anti-corrosion technology of wind turbines has become a key breakthrough. From a solid foundation to a towering tower, from a precise nacelle to a critical blade, and even all mechanical and electrical components, they must maintain stable performance in a highly corrosive environment.

[0003] In response to this, a variety of protection strategies have emerged. Corrosion-resistant materials are known for their excellent protective properties, but their high costs, long R&D cycles and quality control problems limit their widespread application. Although the sacrificial anode method is low-cost and simple in structure, it is limited by a short protection cycle and requires frequent replacement. Impressed current cathodic protection stands out with its advantages of long-term protection and automated control, but the initial investment is large and the maintenance cost is high. Surface modification technology has demonstrated excellent protective effects and strong bonding, but environmental issues cannot be ignored. In contrast, organic coating technology has become the preferred solution in the field of offshore wind power corrosion protection due to its high cost-effectiveness, wide applicability, ease of operation and easy composite properties.

[0004] The core components of offshore wind turbines operating in the marine atmospheric environment, wind turbine blades, are generally constructed of glass fiber reinforced composite materials. The material matrix contains epoxy resin and polyester resin, which itself exhibits a certain degree of corrosion resistance. However, in order to effectively resist surface corrosion caused by salt accumulation in the marine environment and thus ensure the stability of power generation efficiency, it is usually necessary to apply a layer of protective coating on the surface of the blades, such as polyurethane topcoat or polysiloxane topcoat, to enhance its corrosion resistance. In the current market, the mainstream protective coating materials are mostly solvent-based anti-corrosion emulsion coatings, which are known for their excellent solvent resistance and aging resistance. However, its inherent high hardness characteristics can easily cause the coating to peel off when faced with external force impacts in extreme marine environments, thereby exposing the substrate and weakening the protective effectiveness of the blades.

[0005] In view of the continuous improvement of environmental awareness and the in-depth implementation of the sustainable development strategy, it is particularly important to develop a new water-based anti-corrosion topcoat emulsion that is green, has no volatile organic compound (VOC) emissions, and has excellent wear resistance. The development of this type of new coating aims to achieve significant improvement in hardness and wear resistance while maintaining the high-efficiency anti-corrosion performance of the coating by optimizing the material formula and preparation process, thereby ensuring the long-term stable operation of offshore wind turbine blades and promoting the green and healthy development of the clean energy industry. Summary of the invention

[0006] In view of the shortcomings of the prior art, the present invention provides a water-based anti-corrosion topcoat emulsion for offshore wind turbine blades and a preparation method thereof. An inorganic-organic hybrid emulsion composed of silane-modified hollow nano-silica and acrylate monomers and phosphate monomers is used as the topcoat emulsion to effectively improve the hardness and wear resistance of the coating, and increase the adhesion between the coating and the substrate, so that the coating can effectively resist the erosion of corrosive media such as acids and alkalis.

[0007] To achieve the above objectives, the technical solution of the present invention is implemented through the following technical solutions:

[0008] A water-based anti-corrosion topcoat emulsion for offshore wind turbine blades. The water-based anti-corrosion topcoat emulsion is a hybrid emulsion in which a primer and a pre-emulsion are configured in a ratio of 0.5-2:1.5-6. The primer is composed of the following materials in parts by weight: 10-50 parts of deionized water and 0.01-0.08 parts of an initiator; the pre-emulsion is composed of the following materials in parts by weight: 12-35 parts of an acrylate monomer, 1.5-32 parts of silane-modified hollow silica nanoparticles, 2-8 parts of a phosphate monomer, 0.03-0.5 parts of an initiator, and 20-100 parts of deionized water.

[0009] Preferably, the acrylate monomers are at least two of acrylic acid and acrylates, methacrylic acid, methacrylates, hydroxy acrylates, and hydroxy methacrylates.

[0010] Preferably, the phosphate monomer is at least one of methacryloyloxyethyl phosphate, 2-hydroxyethyl methacrylate phosphate, ethylene glycol methacrylate phosphate, and alkyl acrylate phosphate.

[0011] Preferably, the initiator is at least one of ammonium persulfate (APS), potassium persulfate (KPS), azobisisobutyronitrile (AIBN) or azobiscyanovaleric acid (ACVA).

[0012] The preparation method of the water-based anti-corrosion topcoat emulsion for offshore wind turbine blades comprises the following steps:

[0013] (1) Preparation of hollow nano-silica particles:

[0014] After preparing the ethanol solution, add hexadecyltrimethylammonium chloride and stir evenly, then drip triethylamine and stir, control the temperature at 40-60°C, stir and drip ethyl orthosilicate, continue stirring for 1-5h, then control the temperature at 90-150°C to react for 3-10h, cool naturally to room temperature, then disperse in anhydrous ethanol and centrifuge, discard the supernatant, wash the sample with alcohol and then disperse in the extract, centrifuge and filter, repeat the steps of dispersing in the extract and centrifuging 3-5 times to obtain hollow nano silica particles;

[0015] (2) Preparation of silane-modified hollow nano-silica particles:

[0016] The hollow nano-silica particles and the silane coupling agent are dispersed in anhydrous ethanol, and stirred in a constant temperature water bath at 80-120° C. for 0.2-3 hours, and then washed with deionized water and filtered, and the solid part is dried in a vacuum drying oven for 12-24 hours to obtain silane-modified hollow nano-silica particles;

[0017] (3) Preparation of hybrid emulsion:

[0018] Deionized water and an initiator are mixed as a primer; silane-modified hollow nano-silica particles, an initiator, deionized water, and an acrylate monomer and a phosphate monomer are mixed and sheared at a high speed to obtain a pre-emulsion, and after the primer becomes clear and transparent, the pre-emulsion is added dropwise in a semi-continuous manner for 4-6 hours. After the addition is completed, the initiator is added and kept warm for 1-2 hours to obtain a hybrid emulsion.

[0019] Preferably, the ethanol solution in step (1) is prepared by mixing 10-30 mL of water with 1-5 mL of anhydrous ethanol, and the amount of hexadecyltrimethylammonium chloride added is 0.01-1 g, the amount of triethylamine added is 1-10 mL, and the amount of ethyl orthosilicate added is 1-10 mL.

[0020] Preferably, the extract in step (1) is prepared by dissolving 5-20 mL of hydrochloric acid in 10-150 mL of ethanol.

[0021] Preferably, the hollow nano-silica particles prepared in step (1) have a particle size of 15 to 60 nm.

[0022] Preferably, the silane coupling agent in step (2) is at least one of 3-aminopropyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, methyltri(methoxy)silane, 3-propyleneoxypropyltrimethoxysilane and vinyltrimethoxysilane.

[0023] The present invention provides a water-based anti-corrosion topcoat emulsion for offshore wind turbine blades and a preparation method thereof, which has the following advantages over the prior art:

[0024] (1) The water-based anti-corrosion topcoat emulsion for offshore wind turbine blades prepared by the present invention has the high hardness property of hollow nano-silica, which enables the coating to effectively resist wear and tear, thereby extending the service life of the coating;

[0025] (2) The introduction of the phosphate monomer of the present invention significantly enhances the anti-corrosion performance of the emulsion, enabling the coating to resist erosion by a variety of corrosive media;

[0026] (3) The acrylate monomer of the present invention gives the emulsion excellent film-forming properties, making the coating surface smooth and flat, and it is cheap and easy to obtain and has a good appearance effect;

[0027] (4) The topcoat emulsion of the present invention adopts emulsion polymerization, and the solvent is water, which is pollution-free to the environment and meets the requirements of modern green environmental protection. BRIEF DESCRIPTION OF THE DRAWINGS

[0028] Figure 1 This is a TEM image of the silicon-oxygen modified hollow nano-silica particles prepared in Example 1;

[0029] Figure 2 This is a TEM image of the organic-inorganic hybrid topcoat emulsion latex particles prepared in Example 1. DETAILED DESCRIPTION

[0030] In order to make the purpose, technical solution and advantages of the embodiments of the present invention clearer, the technical solution in the embodiments of the present invention is clearly and completely described below in combination with the embodiments of the present invention. Obviously, the described embodiments are part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0031] Embodiment 1:

[0032] Preparation of organic-inorganic hybrid topcoat emulsion:

[0033] (1) Preparation of hollow silica nanoparticles:

[0034] 15 mL of water, 3 mL of anhydrous ethanol, and 0.02 g of hexadecyltrimethylammonium chloride were added to a three-necked flask respectively, and stirred for 20 min. Then, 2 mL of triethylamine was added dropwise, and stirred at room temperature for 20 min. Then, the temperature was controlled at 50°C, and 5 mL of tetraethyl orthosilicate was added dropwise under vigorous stirring, and stirred for reaction for 3 h. Subsequently, the sample was transferred to a high-pressure reactor, and the temperature was controlled at 130°C for reaction for 6 h. The sample was naturally cooled to room temperature, and all samples were dispersed in anhydrous ethanol. The sample was centrifuged at 2500 r / min for 8 min, and the supernatant was discarded. The sample was dissolved in 50 mL of ethanol with 8 mL of hydrochloric acid to prepare an extract. The sample after alcohol washing was dispersed in a small amount of extract by ultrasonication for 10 min, and centrifugation was performed. The sample was repeated 3 times to remove the template. Finally, the sample was ultrasonically dispersed in anhydrous ethanol to obtain hollow nano-silica particles with a diameter of 30 nm.

[0035] (2) Preparation of silicon-oxygen modified hollow nano-silica particles:

[0036] The hollow silica nanoparticles and vinyl trimethoxysilane in (1) were dispersed in anhydrous ethanol and stirred in a constant temperature water bath at 70°C for 2 hours, then washed with deionized water and filtered, and the solid part was dried in a vacuum drying oven for 12 hours to obtain silane-modified hollow silica nanoparticles (such as Figure 1 );

[0037] (3) Preparation of organic-inorganic hybrid topcoat emulsion:

[0038] Deionized water and initiator APS are used as primers, and the silicon-oxygen modified hollow nano-silica particles prepared in (2), initiator APS, deionized water and methyl methacrylate (MMA), butyl acrylate (BA), and 2-hydroxyethyl methacrylate phosphate are mixed in a mass ratio of 50:48:2 and sheared at high speed to obtain a pre-emulsion. After the primer becomes clear and transparent, the pre-emulsion is added dropwise in a semi-continuous manner for 4 hours, and then kept warm for 1 hour. The mass percentage of the primer and the pre-emulsion is 70:30, and an organic-inorganic hybrid topcoat emulsion is obtained.

[0039] Embodiment 2:

[0040] Preparation of organic-inorganic hybrid topcoat emulsion:

[0041] (1) Preparation of hollow silica nanoparticles:

[0042] Add 20mL of water, 5mL of anhydrous ethanol, and 0.03g of hexadecyltrimethylammonium chloride to a three-necked flask, stir for 20min, then drop 3mL of triethylamine, stir at room temperature for 20min, then control the temperature at 50℃, under vigorous stirring, drop 45mL of ethyl orthosilicate, and stir for 3h. Then transfer the sample to a high-pressure reactor, control the temperature at 130℃ to react for 6h, cool naturally to room temperature, and disperse all samples in anhydrous ethanol, centrifuge at 2500r / min for 8min, discard the supernatant, dissolve in 50mL of ethanol with 8mL of hydrochloric acid to make an extract, disperse the alcohol-washed sample into a small amount of extract by ultrasonication for 10min, centrifuge and filter, repeat 3 times to remove the template, and finally ultrasonically disperse the sample into anhydrous ethanol to obtain hollow nano-silica particles with a diameter of 40nm;

[0043] (2) Preparation of silicon-oxygen modified hollow nano-silica particles:

[0044] The hollow silica nanoparticles and 3-propyleneoxypropyltrimethoxysilane were dispersed in anhydrous ethanol and stirred in a constant temperature water bath at 125°C for 2.5 hours, then washed with deionized water and filtered, and the solid part was dried in a vacuum drying oven for 36 hours to obtain silicon-oxygen modified hollow nano-silica particles.

[0045] (3) Preparation of organic-inorganic hybrid topcoat emulsion:

[0046] Deionized water and initiator KPS are used as primers. The silicon-oxygen-modified hollow nano-silica particles prepared in (2), initiator KPS, deionized water, isooctyl acrylate (HMA), BA, and ethylene glycol methacrylate phosphate are mixed in a mass ratio of 45:50:5 and sheared at high speed to obtain a pre-emulsion. After the primer becomes clear and transparent, the pre-emulsion is added dropwise in a semi-continuous manner. The addition time is 3.5 hours and the temperature is kept warm for 1.5 hours. The mass percentage of the primer and the pre-emulsion is 70:30, thereby obtaining an organic-inorganic hybrid topcoat emulsion.

[0047] Embodiment 3:

[0048] Preparation of organic-inorganic hybrid topcoat emulsion:

[0049] (1) Preparation of hollow silica nanoparticles:

[0050] Add 15mL water, 5mL anhydrous ethanol, 0.05g hexadecyltrimethylammonium chloride to a three-necked flask, stir for 10min, then drop 10mL triethylamine, stir at room temperature for 30min, then control the temperature at 60℃, under vigorous stirring, drop 5mL ethyl orthosilicate, stir and react for 5h. Then transfer the sample to a high-pressure reactor, control the temperature at 150℃ to react for 10h, cool naturally to room temperature, and disperse all samples in anhydrous ethanol, centrifuge at 3000r / min for 10min, discard the supernatant, dissolve 20mL hydrochloric acid in 100mL ethanol to make an extract, disperse the alcohol-washed sample in a small amount of extract by ultrasonic for 30min, centrifuge and filter, repeat 3 times to remove the template, and finally ultrasonically disperse the sample in anhydrous ethanol to obtain hollow nano-silica particles with a diameter of 50nm.

[0051] (2) Preparation of silicon-oxygen modified hollow nano-silica particles:

[0052] The hollow silica nanoparticles and γ-glycidyloxypropyltrimethoxysilane were dispersed in anhydrous ethanol and stirred in a constant temperature water bath at 95°C for 2 hours, then washed with deionized water and filtered, and the solid part was dried in a vacuum drying oven for 30 hours to obtain silicon-oxygen modified hollow nano-silica particles.

[0053] (3) Preparation of organic-inorganic hybrid topcoat emulsion:

[0054] Deionized water and initiator ACVA are used as primers, and the silicon-oxygen modified hollow nano-silica particles prepared in (2), initiator ACVA, deionized water and methyl acrylate (MA), isooctyl hydroxymethacrylate (OEHMA), and ethylene glycol methacrylate phosphate are mixed in a mass ratio of 45:50:5 and sheared at high speed to obtain a pre-emulsion. After the primer becomes clear and transparent, the pre-emulsion is added dropwise in a semi-continuous manner for 3 hours, and then kept warm for 1.5 hours. The mass percentage of the primer and the pre-emulsion is 70:30, and an organic-inorganic hybrid topcoat emulsion is obtained.

[0055] Comparative Example 1:

[0056] Preparation of hybrid emulsion:

[0057] Deionized water and initiator APS are used as primers. Initiator APS, deionized water and methyl methacrylate (MMA), butyl acrylate (BA), and 2-hydroxyethyl methacrylate phosphate are mixed in a mass ratio of 0.06:182:50:48:2 and sheared at high speed to obtain a pre-emulsion. After the primer becomes clear and transparent, the pre-emulsion is added dropwise in a semi-continuous manner for 4 hours, and then kept warm for 1 hour. The mass percentage of the primer and the pre-emulsion is 70:30 to obtain a hybrid emulsion.

[0058] Comparative Example 2:

[0059] Preparation of hybrid emulsion:

[0060] Deionized water and initiator KPS were used as primers, and the modified hollow nano-silica particles prepared in Example 2, initiator KPS, deionized water and isooctyl acrylate (HMA), BA in a mass ratio of 2:0.06:185:50:50 were mixed and sheared at high speed to obtain a pre-emulsion. After the primer became clear and transparent, the pre-emulsion was added dropwise in a semi-continuous manner. The addition time was 3.5 hours and then kept warm for 1.5 hours. The mass percentage of the primer and the pre-emulsion was 70:30, and a hybrid emulsion was obtained.

[0061] Paint matching and testing:

[0062] 1. Add 2 g of dispersant BYK-190, 0.5 g of wetting agent TEGO4100, 0.5 g of defoamer BYK-1711 and 0.5 g of flash rust preventer Halox Hash-X150 to 100 g of the emulsion prepared in Examples 1-3 and Comparative Examples 1-2, stir at low speed, then add 20 g of titanium dioxide, 5 g of pigment and 1 g of thickener Dow ACRYSOL RM-8W, and then spray on the blades with primer and intermediate paint with a spray gun. The test results are shown in Table 1.

[0063] 2. The free formaldehyde content of the composite emulsions prepared in Examples 1-5 and Comparative Example 1 was tested according to the free formaldehyde content standard GB18583-2008. The test results are shown in Table 1.

[0064] 3. The composite emulsions prepared in Examples 1-5 and Comparative Example 1 were vacuum dried at 50°C for 10 hours and then dried at 120°C for 1 hour. The whiteness value of the obtained latex film was tested on a whiteness meter TC-BD48B. The test results are shown in Table 1.

[0065] 4. Take 1 ml of the composite emulsion prepared in Examples 1-5 and Comparative Example 1 every 20 minutes and test the sugar content with a sugar meter PAL-1. Record the time required when the sugar content of the composite emulsion does not change. The recorded results are shown in Table 1.

[0066] Table 1

[0067]

[0068]

[0069] It can be seen from the data in the table that the adhesion, wear resistance, impact resistance, aging resistance, salt spray resistance, and moisture and heat resistance of the topcoat in Examples 1-3 are all higher than those in Comparative Examples 1 and 2, indicating that the introduction of silane-modified hollow silica nanoparticles and phosphate monomers improves the wear resistance and corrosion resistance of the water-based hybrid emulsion topcoat.

[0070] The above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit the same. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that the technical solutions described in the aforementioned embodiments may still be modified, or some of the technical features may be replaced by equivalents. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present invention.

Claims

1. A water-based anti-corrosion topcoat emulsion for offshore wind turbine blades, characterized in that: The water-based anticorrosive topcoat emulsion is a hybrid emulsion in which a primer and a pre-emulsion are configured in a ratio of 0.5-2:1.5-6. The primer is composed of the following substances in parts by weight: 10-50 parts of deionized water and 0.01-0.08 parts of an initiator; the pre-emulsion is composed of the following substances in parts by weight: 12-35 parts of an acrylate monomer, 1.5-32 parts of silane-modified hollow silica nanoparticles, 2-8 parts of a phosphate monomer, 0.03-0.5 parts of an initiator, and 20-100 parts of deionized water.

2. The water-based anticorrosive topcoat emulsion according to claim 1, characterized in that: The acrylic acid ester monomers are at least two of acrylic acid and acrylic acid esters, methacrylic acid, methacrylic acid esters, hydroxy acrylic acid esters, and hydroxy methacrylic acid esters.

3. The water-based anticorrosive topcoat emulsion according to claim 1, characterized in that: The phosphate monomer is at least one of methacryloyloxyethyl phosphate, 2-hydroxyethyl methacrylate phosphate, ethylene glycol methacrylate phosphate, and alkyl acrylate phosphate.

4. The water-based anticorrosive topcoat emulsion according to claim 1, characterized in that: The initiator is at least one of ammonium persulfate, potassium persulfate, azobisisobutyronitrile or azobiscyanovaleric acid.

5. A method for preparing the water-based anticorrosive topcoat emulsion as claimed in any of claims 1 to 4, characterized in that: The preparation method comprises the following steps: (1) Preparation of hollow nano-silica particles: After preparing the ethanol solution, add hexadecyltrimethylammonium chloride and stir evenly, then drip triethylamine and stir, control the temperature at 40-60°C, stir and drip ethyl orthosilicate, continue stirring for 1-5h, then control the temperature at 90-150°C to react for 3-10h, cool naturally to room temperature, then disperse in anhydrous ethanol and centrifuge, discard the supernatant, wash the sample with alcohol and then disperse in the extract, centrifuge and filter, repeat the steps of dispersing in the extract and centrifuging 3-5 times to obtain hollow nano silica particles; (2) Preparation of silane-modified hollow nano-silica particles: The hollow nano-silica particles and the silane coupling agent are dispersed in anhydrous ethanol, and stirred in a constant temperature water bath at 80-120° C. for 0.2-3 hours, and then washed with deionized water and filtered, and the solid part is dried in a vacuum drying oven for 12-24 hours to obtain silane-modified hollow nano-silica particles; (3) Preparation of hybrid emulsion: Deionized water and an initiator are mixed as a primer; silane-modified hollow nano-silica particles, an initiator, deionized water, and an acrylate monomer and a phosphate monomer are mixed and sheared at a high speed to obtain a pre-emulsion, and after the primer becomes clear and transparent, the pre-emulsion is added dropwise in a semi-continuous manner for 4-6 hours. After the addition is completed, the initiator is added and kept warm for 1-2 hours to obtain a hybrid emulsion.

6. The preparation method according to claim 5, characterized in that: In the step (1), the ethanol solution is prepared by mixing 10-30 mL of water with 1-5 mL of anhydrous ethanol, and the amount of hexadecyltrimethylammonium chloride added is 0.01-1 g, the amount of triethylamine added is 1-10 mL, and the amount of ethyl orthosilicate added is 1-10 mL.

7. The preparation method according to claim 5, characterized in that: The extract in step (1) is prepared by dissolving 5-20 mL of hydrochloric acid in 10-150 mL of ethanol.

8. The preparation method according to claim 5, characterized in that: The hollow nano-silica particles prepared in step (1) have a particle size of 15 to 60 nm.

9. The preparation method according to claim 5, characterized in that: The silane coupling agent in step (2) is at least one of 3-aminopropyltrimethoxysilane, γ-glycidyloxypropyltrimethoxysilane, methyltri(methoxy)silane, 3-propyleneoxypropyltrimethoxysilane and vinyltrimethoxysilane.

Citation Information

Patent Citations

  • In-situ nano hybridization styrene-acrylic emulsion and rust-resisting paint using the emulsion as base material

    CN104892816A

  • Green water-based emulsion with high activity, zero residue and excellent anti-yellowing performance and preparation method thereof

    CN118755013A