Preparation method of convenient spraying type antibacterial transparent coating
By using antibacterial spraying compositions composed of Ag elements, Co elements, tannic acid and polyvinylpyrrolidone, the problems of complex processes and toxic solvents in the prior art are solved, and efficient transparent antibacterial coating without drying under low temperature conditions is achieved. simplifies the process and improves safety and environmental protection.
Patent Information
- Application Number
- CN202411271578.0
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-11
AI Technical Summary
The existing antibacterial coating technology has complex processes, needs to be dried and cured and used toxic solvents, which limits its large-scale application and safety and convenience.
An antibacterial spraying composition is provided, consisting of Ag elements, Co elements, tannic acid and polyvinylpyrrolidone, and a coating is formed by spraying, without subsequent heating and drying, and does not contain highly toxic reagents, and has high transparency and antibacterial properties.
It realizes the formation of an efficient transparent antibacterial coating without additional treatment under low temperature conditions, simplifies the process, reduces costs, improves safety and environmental protection, while maintaining good antibacterial effect and adhesion.
Smart Images

Figure HDA0005038870410000011 
Figure HDA0005038870410000021 
Figure HDA0005038870410000022
Abstract
Description
Technical Field
[0001] The present application relates to an antibacterial coating preparation technology, and specifically to an antibacterial composition for conveniently preparing a spray-type antibacterial transparent coating and a preparation method thereof. Background Art
[0002] With the frequent occurrence of public health events, the problem of bacterial resistance is becoming increasingly serious. Applying antibacterial coatings on the surface of susceptible objects can block the indirect contact transmission chain between microorganisms and human surfaces, reduce the frequent use of short-term disinfection agents, and reduce the probability of the emergence of bacterial resistance genes.
[0003] For example, Chinese patent application publication number CN117844274A discloses a low-temperature synthesis method for a long-lasting self-disinfecting coating, the steps of which are as follows: (1) Stable aqueous Ag + -(Ti(O2))2-complex precursor solution preparation; (2) Ag+-(Ti(O2)) spraying; (3) drying and curing the Ag+-(Ti(O2))2-complex precursor solution prepared in the above steps on a non-high temperature treatment substrate to obtain a non-high temperature treatment substrate with a low temperature deposited nano silver-titanium dioxide coating. This application deposits a visible light absorbing nano silver-titanium dioxide coating on the surface of a non-high temperature treatment substrate at a low temperature. However, the sprayed antibacterial coating of this method requires drying, curing and other treatments.
[0004] In the existing antibacterial coating technology, there are problems such as complex processes and the use of toxic solvents, which limit its large-scale application. Therefore, the current safe and convenient preparation method of antibacterial coating needs to be further improved. Summary of the invention
[0005] On the one hand, the present application provides an antibacterial spray composition, which can be sprayed onto an object to be coated to form a coating without the need for subsequent heating, drying, curing and other processes.
[0006] On the other hand, the antibacterial spray composition provided in the present application does not contain highly toxic agents, and the antibacterial coating is more environmentally friendly.
[0007] In another aspect, the present application provides an antibacterial spray composition, which is sprayed onto an object to form a coating having high antibacterial properties and high transparency, and in particular, has high antibacterial properties under low temperature conditions.
[0008] A mixed liquid of an antibacterial spray composition is formed by Ag element, Co element, tannic acid and polyvinyl pyrrolidone, and the pH value of the mixed liquid is 5-9.
[0009] The mass ratio of tannic acid to polyvinyl pyrrolidone is 1:(2.5-4).
[0010] The mixed liquid forms an antibacterial coating on the object by spraying. During the coating formation process, no additional heating, drying and curing is required, and it can be air-dried under natural conditions. The coating has high transparency and good antibacterial effect.
[0011] A method for preparing a mixed liquid of an antibacterial spray composition comprises: mixing tannic acid and polyvinyl pyrrolidone into a first mixed solution; mixing the first mixed solution with a soluble cobalt salt and a soluble silver salt to form a second mixed liquid; and adjusting the pH of the second mixed liquid to 5-9 to obtain a mixed liquid of the antibacterial spray composition.
[0012] The mass ratio of tannic acid to polyvinyl pyrrolidone is 1:(2.5-4).
[0013] The mixed liquid of the antibacterial spray composition is sprayed on an object to form an antibacterial coating, which has high transparency and good antibacterial effect. BRIEF DESCRIPTION OF THE DRAWINGS
[0014] Figure 1 This is a scanning electron microscope (SEM) image of the coating prepared in Example 1 of the present invention;
[0015] FIG. 2( a ) and FIG. 2( b ) are AFM images of the coating prepared in Example 1 of the present invention and their corresponding height profiles;
[0016] FIG3(a) and FIG3(b) are graphs showing the removal rate of Escherichia coli by the coating prepared in Example 1 of the present invention at room temperature and the corresponding colony graphs;
[0017] FIG. 4( a ) and FIG. 4( b ) are graphs showing the removal rate of Escherichia coli at low temperature by the coating prepared in Example 1 of the present invention and the corresponding colony graphs. DETAILED DESCRIPTION
[0018] The mixed solution of the antibacterial spray composition of the present invention and its preparation method are further described in detail below. The protection scope of this application is not limited, and its protection scope is defined by the claims. Certain disclosed specific details provide a comprehensive understanding of each disclosed embodiment. However, those skilled in the relevant art know that the embodiment can be implemented without using one or more of these specific details and using other materials, etc.
[0019] Unless the context requires otherwise, in the specification and claims, the terms "include" and "comprising" should be construed as having an open-ended, inclusive meaning, that is, "including, but not limited to".
[0020] The "embodiment", "one embodiment", "another embodiment" or "certain embodiments" mentioned in the specification means that the specific features, structures or characteristics described in connection with the embodiment are included in at least one embodiment. Therefore, "embodiment", "one embodiment", "another embodiment" or "certain embodiments" do not necessarily all refer to the same embodiment. And the specific features, structures or characteristics can be combined in any way in one or more embodiments. Each feature disclosed in the specification can be replaced by any alternative feature that can provide the same, equal or similar purpose. Therefore, unless otherwise specified, the disclosed features are only general examples of equal or similar features.
[0021] The present invention will be further described below in conjunction with specific examples. It should be understood that these examples are intended only to illustrate the present invention and are not intended to limit the scope of the present invention. The experimental methods in the following examples without specifying specific conditions are usually performed under normal conditions or according to the conditions recommended by the manufacturer. Unless otherwise stated, all percentages, ratios, proportions, or parts are by weight.
[0022] The units of weight-volume percentage in the present invention are well known to those skilled in the art, for example, refer to the weight of the solute in 100 ml of solution.
[0023] In the present invention, the concentration unit "M" of a solution represents mol / L.
[0024] In the prior art, the antibacterial liquid coated on the object by spraying usually contains toxic agents, or the antibacterial liquid is not easy to form a coating by spraying, or the process of forming the coating must be relatively complicated, and sometimes the coating has low transparency, etc. The antibacterial spray composition provided by the present application can overcome at least one of the above problems.
[0025] The mixed liquid of the antibacterial spray composition of the present application can be coated on the surface of objects made of materials such as glass, stainless steel, hard paper, or resin.
[0026] On the one hand, a mixed liquid of an antibacterial spray composition is provided, wherein the mixed liquid is formed by Ag element, Co element, tannic acid and polyvinyl pyrrolidone, and the pH value of the mixed liquid is 5-9.
[0027] The mass ratio of tannic acid to polyvinyl pyrrolidone is 1:(2.5-4).
[0028] In the mixed solution, tannic acid and polyvinyl pyrrolidone are interwoven into a uniform and dense three-dimensional grid structure under the above conditions, which can evenly disperse the antibacterial metal elements Ag and Co in the three-dimensional grid structure, ensuring the sustained release of the antibacterial metals and further improving the antibacterial cycle. +and nanosilver. Co exists in ionic form.
[0029] The mixed liquid is coated on the object by spraying, and the coating has high transparency and good antibacterial effect in the final case.
[0030] In certain embodiments, the pH of the mixture is 5-6.5.
[0031] When the pH value of the mixed solution of the antibacterial spray composition is 5-6.5 and the temperature is low, the Ag element in the mixed solution is mainly converted into Ag under the action of the Co element, tannic acid and polyvinyl pyrrolidone. + Therefore, the coating formed by spraying the mixed liquid onto the object still maintains good antibacterial properties and transparency under low temperature conditions (such as around 4°C).
[0032] As an option, the pH of the mixed solution is about 5.0-6.0.
[0033] In certain embodiments, the mass ratio of tannic acid to polyvinyl pyrrolidone is 1:3.
[0034] In the mixed liquid of the present application, especially by controlling the ratio of tannic acid to polyvinyl pyrrolidone at 1:3, the coating has good wear resistance while ensuring good antibacterial properties and transparency at room temperature and low temperature.
[0035] The molecular weight of the polyvinyl pyrrolidone of the present application is 30,000-40,000.
[0036] In certain embodiments, in the mixed solution, the molar ratio of the cobalt element to the silver element is (6-14):1.
[0037] In the above-mentioned mixed solution, the ratio of the amount of cobalt element to the amount of silver element is controlled within the range of (6-14):1, which can form an antibacterial coating that takes both cost and high activity into consideration.
[0038] The ratio of the amount of cobalt to silver is controlled to be within the range of (6-14):1. Especially in low temperature environments, the presence of Co ions plays a role in regulating Ag + The effect of content on Ag 0 Oxidized to Ag + The coating formed by coating the mixed liquid of the antibacterial spray composition on the material has good antibacterial performance and transparency. If the silver content is too high, the more silver is, the easier it is to agglomerate at low temperatures, which is not conducive to the release of silver ions.
[0039] The mass ratio of Ag element to tannic acid is (0.01-0.04):1.
[0040] In a low-temperature environment, the silver content cannot be too high, otherwise it will be reduced by tannic acid to a larger amount of nano-silver, resulting in poor low-temperature antibacterial effect.
[0041] As an alternative, in the mixed solution, the mass ratio of cobalt element to silver element is about (11-12):1, pH=7, and the mass ratio of Ag element to tannic acid is about 0.04:1. The coating formed by spraying the mixed solution onto the object still maintains good antibacterial properties and transparency under low temperature conditions (such as around 4°C).
[0042] The concentration of the mixed solution can be adjusted according to actual needs.
[0043] The solvent of the mixed solution can be water.
[0044] The coating formed by spraying the mixed liquid of the above antibacterial spray composition can have a coating thickness that can be adjusted according to actual conditions.
[0045] For example, the coating thickness is 8nm-267nm; the coating absorbance is 0.05-0.5.
[0046] In order to ensure that the thickness and morphology of the formed coating are similar, the spraying angle and time are fixed during spraying.
[0047] The coating formed by spraying the mixed liquid of the antibacterial spray composition provided in the present application can maintain a good antibacterial effect under normal temperature and low temperature conditions. The coating has good adhesion and durability, and provides reliable protection for the surface of the object.
[0048] In addition, the mixed liquid of the antibacterial spray composition can be directly sprayed on the surface of the object and air-dried under natural conditions without the need for additional heating, drying and curing, making the coating process simpler.
[0049] on the other hand, The preparation method of the mixed liquid of the above-mentioned antibacterial spray composition includes: mixing tannic acid and polyvinyl pyrrolidone into a first mixed solution; mixing the first mixed solution with a soluble cobalt salt and a soluble silver salt to form a second mixed solution; adjusting the pH of the second mixed solution to 5-9 to obtain the mixed liquid of the antibacterial spray composition.
[0050] The mass ratio of tannic acid to polyvinyl pyrrolidone is 1:(2.5-4).
[0051] Soluble cobalt salts include cobalt nitrate; soluble silver salts include silver nitrate. The choice of salts has no essential effect on the final antibacterial effect, as long as the corresponding silver ions and cobalt ions can be provided.
[0052] The pH can be adjusted with alkaline substances such as sodium hydroxide.
[0053] In certain embodiments, the mixed solution is prepared in dark conditions.
[0054] Under dark conditions, in the second mixed solution, the rate at which tannic acid reduces silver ions to nanosilver is slow, or even inhibits the reduction of silver ions to nanosilver, thereby preventing the formation of large silver particle clusters. Therefore, the antibacterial mixed solution of the present application also has a good antibacterial effect at low temperatures.
[0055] The dark condition described in this application refers to an environment with dim light.
[0056] The coating sprayed with the mixed liquid of the antibacterial spray composition of the present application has simple and fast steps during the spraying process, and only requires one or two sprayings, without complicated equipment and operations, making it more convenient and easy to implement, saving time and cost. Secondly, the use of safe and non-toxic tannic acid and polyvinyl pyrrolidone avoids the use of toxic solvents, which is beneficial to protecting the environment and the health of users. Thirdly, the mixed liquid of the antibacterial spray composition of certain embodiments effectively improves the antibacterial properties of the coating in a low temperature environment, can effectively inhibit bacterial growth, and reduce the risk of cross infection. In addition, the prepared coating has high transparency, not only can it maintain the original color and texture of the surface of the object, but also has good adhesion and durability, can maintain the antibacterial effect for a long time under normal temperature and low temperature environment, and provide reliable protection for the surface of the object. In summary, this method is superior to traditional technology in many aspects and has broad application prospects and market potential.
[0057] The mixed solution of the antibacterial spray composition of the present invention and its efficacy are further described below in conjunction with specific examples. The substances used in the following examples are all chemically pure.
[0058] The calculation formula of the antibacterial rate in the following embodiment is:
[0059] The calculation formula of antibacterial rate is:
[0060] R(%)=(A–B) / B×100%
[0061] Where: R——antibacterial rate (%)
[0062] A——Average bacterial count of blank group (CFU / sample)
[0063] B——Average bacterial colony count of antibacterial sample group (CFU / sample)
[0064] When the R value reaches or exceeds 90%, the sample is deemed to show antibacterial activity.
[0065] The mechanical stability analysis of the coating is carried out with the aid of a sandpaper friction test. The coated glass sheet (2cm×2cm) is placed face down on 800-grit sandpaper, and a 100g weight is placed on the back to apply pressure. The sample is then pushed to slide 20cm in a straight line, and then the sample is rotated 90° and the process is repeated. This sliding and rotating action is defined as a complete sandpaper friction test cycle, and the sample is required to maintain a moving speed of approximately 1cm / s in each cycle. After completing the predetermined number of cycles, the test can be stopped, and normal temperature and low temperature film-sticking experiments can be carried out to test the inhibition rate of the coating on Escherichia coli to evaluate its antibacterial effect after wear.
[0066] Example 1
[0067] Preparation of mixed solution of antibacterial spray composition
[0068] Step 1: weigh 0.15 g of polyvinyl pyrrolidone (povidone K30) powder and dissolve it in 10 mL of water in the dark. After stirring evenly, add 0.05 g of tannic acid powder and stir to obtain a milky white clear and transparent solution.
[0069] Step 2: add 100 μL of 0.1 mol / L silver nitrate solution and 0.03 g of cobalt nitrate powder to the solution in step 1, and stir evenly to obtain a pink solution.
[0070] Step 3: add 1 mol / L sodium hydroxide solution to the solution in step 2, adjust the pH to 5, and stir for 3 hours to obtain a mixed solution of the antibacterial spray composition.
[0071] Preparation of the coating: spray the obtained mixed liquid of the antibacterial spray composition on a glass sheet, and obtain a finished coating product after natural air drying.
[0072] The antibacterial rate of the coating sample obtained in this example was 100% at room temperature (25°C) on the seventh day, and 97.9% at low temperature (4°C) on the seventh day. After ten sandpaper friction tests, the antibacterial rates at room temperature and low temperature were 98.7% and 98.6% respectively, and the absorbance in the range of 300-1000nm was 0.4-0.5.
[0073] The coating of this embodiment was analyzed by scanning electron microscopy (SEM), the electron microscope model was XL30ESEM-TMP (Poland), and the accelerating voltage was 3 kV. The results are shown in the attached Figure 1 As shown, the coating is uniform and dense, and the formed silver clusters are small.
[0074] The coating of this embodiment was subjected to atomic force microscopy (AFM) analysis, and the results are shown in Figures 2(a) and 2(b). Figure 2(a) shows that the coating surface is uniform; in Figure 2(b), the horizontal axis is the lateral size of the coating, and the vertical axis is the coating thickness. The thickness of the coating is relatively uniform.
[0075] For the antibacterial test diagram of the coating of this embodiment at room temperature, refer to Figure 3(a) , 3(b) ; Antibacterial test chart at low temperature, reference Figure 4(a) , 4(b) .
[0076] exist Figure 3(a) and 4(a) The values 5, 6, 7, 8, and 9 in the figure respectively represent the pH values of the mixed solution of the antibacterial spray composition. As shown in Figure 3(a), the antibacterial rate of the coating at room temperature gradually decreases with time within seven days, but is generally higher than 95%, and the antibacterial effect under acidic conditions is better than that under alkaline conditions. Figure 3(b) and 4(a) In the figure, N-Ag2Co3-5 indicates that the pH of the mixed solution of the antibacterial spray composition is 5, and so on, it shows how many bacteria the coating has every day. As shown in Figure 3(b), the antibacterial rate of the coating at room temperature (25°C) gradually decreases with time within seven days, and the antibacterial effect is better under acidic conditions.
[0077] As shown in Figure 4(a), compared with room temperature, the low-temperature antibacterial rate of the coating decreased significantly within seven days, but the antibacterial effect under acidic conditions was still better than that under alkaline conditions. As shown in Figure 4(b), the low-temperature (4°C) antibacterial rate of the coating decreased gradually with time within seven days, but the antibacterial effect under acidic conditions was better.
[0078] Example 2
[0079] The preparation steps are as follows:
[0080] Step 1: weigh 0.12 g of polyvinyl pyrrolidone (povidone K30) powder and dissolve it in 10 mL of water in the dark. After stirring evenly, add 0.04 g of tannic acid powder and stir to obtain a milky white clear and transparent solution.
[0081] Step 2: add 150 μL of 0.1 mol / L silver nitrate solution and 0.05 g of cobalt nitrate powder to the solution in step 1, and stir evenly to obtain a pink solution.
[0082] Step 3: add 1 mol / L sodium hydroxide solution to the solution in step 2, adjust the pH to 6.5 and stir for 3 hours.
[0083] Step 4: Spray the solution in step 3 onto the glass sheet and allow it to dry naturally to obtain a finished coating product.
[0084] The coating sample obtained in this example has an antibacterial rate of 100% on the seventh day at room temperature (25°C) and a 100% antibacterial rate on the seventh day at low temperature (4°C). After ten sandpaper friction tests, the antibacterial rates at room temperature and low temperature are 99.8% and 99.6% respectively, and the absorbance in the range of 300-1000nm is 0.4-0.5.
[0085] Example 3
[0086] The preparation steps are as follows:
[0087] Step 1: weigh 0.18 g of polyvinyl pyrrolidone (povidone K30) powder and dissolve it in 10 mL of water in the dark. After stirring evenly, add 0.04 g of tannic acid powder and stir to obtain a milky white clear and transparent solution.
[0088] Step 2: add 50 μL of 0.1 mol / L silver nitrate solution and 0.02 g of cobalt nitrate powder to the solution in step 1, and stir evenly to obtain a pink solution.
[0089] Step 3: add 1 mol / L sodium hydroxide solution to the solution in step 2, adjust the pH to 8 and stir for 3 hours.
[0090] Step 4: Spray the solution in step 3 onto the glass sheet and allow it to dry naturally to obtain a finished coating product.
[0091] The antibacterial rate of the coating sample obtained in this example was 83.9% on the seventh day at room temperature and 72.4% on the seventh day at low temperature. After ten sandpaper friction tests, the antibacterial rates at room temperature and low temperature were 77.8% and 65.3% respectively, and the absorbance in the range of 300-1000nm was 0.1-0.35.
[0092] Example 4
[0093] The preparation steps are as follows:
[0094] Step 1: weigh 0.24 g of polyvinyl pyrrolidone (povidone K30) powder and dissolve it in 10 mL of water in the dark. After stirring evenly, add 0.08 g of tannic acid powder and stir to obtain a milky white clear and transparent solution.
[0095] Step 2: add 200 μL of 0.1 mol / L silver nitrate solution and 0.05 g of cobalt nitrate powder to the solution in step 1, and stir evenly to obtain a pink solution.
[0096] Step 3: add 1 mol / L sodium hydroxide solution to the solution in step 2, adjust the pH to 9 and stir for 3 hours.
[0097] Step 4: Spray the solution in step 3 onto the glass sheet and allow it to dry naturally to obtain a finished coating product.
[0098] The antibacterial rate of the coating sample obtained in this example was 100% on the seventh day at room temperature (25°C) and 86.7% on the seventh day at low temperature (4°C). After ten sandpaper friction tests, the antibacterial rates at room temperature and low temperature were 67.5% and 53.1% respectively, and the absorbance in the range of 300-1000nm was 0.1-0.5.
[0099] Comparative Example 1
[0100] Preparation of mixed solution of antibacterial spray composition
[0101] Step 1: weigh 0.15 g of polyvinyl pyrrolidone powder and dissolve it in 10 mL of water in the dark. After stirring evenly, add 0.05 g of tannic acid powder and stir to obtain a milky white clear and transparent solution.
[0102] Step 2: add 100 μL of 0.1 mol / L silver nitrate solution and 0.03 g of ferric nitrate powder to the solution in step 1, and stir evenly to obtain a pink solution.
[0103] Step 3: add 1 mol / L sodium hydroxide solution to the solution in step 2, adjust the pH to 5, and stir for 3 hours to obtain a mixed solution of the antibacterial spray composition.
[0104] Preparation of the coating: spray the obtained mixed liquid of the antibacterial spray composition on a glass sheet, and obtain a finished coating product after natural air drying.
[0105] The antibacterial rate of the coating sample obtained in this example was 98.7% at room temperature (25°C) on the seventh day, and 83.4% at low temperature (4°C) on the seventh day. After ten sandpaper friction tests, the antibacterial rates at room temperature and low temperature were 94.2% and 86.9% respectively, and the absorbance in the range of 300-1000nm was 0.4-0.5.
[0106] Comparative Example 2
[0107] Preparation of mixed solution of antibacterial spray composition
[0108] Step 1: weigh 0.15 g of polyvinyl pyrrolidone powder (povidone K30) and dissolve it in 10 mL of water in the dark. After stirring evenly, add 0.15 g of tannic acid powder and stir to obtain a milky white clear and transparent solution.
[0109] Step 2: add 100 μL of 0.1 mol / L silver nitrate solution and 0.03 g of cobalt nitrate powder to the solution in step 1, and stir evenly to obtain a pink solution.
[0110] Step 3: add 1 mol / L sodium hydroxide solution to the solution in step 2, adjust the pH to 5, and stir for 3 hours to obtain a mixed solution of the antibacterial spray composition.
[0111] Preparation of the coating: spray the obtained mixed liquid of the antibacterial spray composition on a glass sheet, and obtain a finished coating product after natural air drying.
[0112] The antibacterial rate of the coating sample obtained in this example was 100% at room temperature (25°C) on the seventh day, and 95.3% at low temperature (4°C) on the seventh day. After ten sandpaper friction tests, the antibacterial rates at room temperature and low temperature were 72.6% and 40.3% respectively, and the absorbance in the range of 300-1000nm was 0.5-0.6.
[0113] Comparative Example 3
[0114] Preparation of mixed solution of antibacterial spray composition
[0115] Step 1: weigh 0.15 g of polyvinyl pyrrolidone powder (povidone K30) and dissolve it in 10 mL of water in the dark. After stirring evenly, add 0.15 g of tannic acid powder, 100 μL of 0.1 mol / L silver nitrate solution and 0.03 g of cobalt nitrate powder, and stir to obtain a solution with flocs.
[0116] Step 2: Add 1 mol / L sodium hydroxide solution to the solution in step 2, adjust the pH to 5, and stir for 3 hours to obtain a mixed solution of the antibacterial spray composition.
[0117] Preparation of coating: spray the obtained mixed liquid of antibacterial spray composition on a glass sheet, and obtain the finished coating after natural air drying. The uniformity of the coating is poor.
[0118] The antibacterial rate of the coating sample obtained in this example was 100% at room temperature (25°C) on the seventh day, and 86.7% at low temperature (4°C) on the seventh day. After ten sandpaper friction tests, the antibacterial rates at room temperature and low temperature were 53.4% and 20.8% respectively, and the absorbance in the range of 300-1000nm was 0.6-0.7.
Claims
1. A mixed solution of an antibacterial spray composition, the mixed solution is formed by Ag element, Co element, tannic acid and polyvinyl pyrrolidone, and the pH value of the mixed solution is 5-9.
2. The mixed solution according to claim 1, characterized in that The mass ratio of tannic acid to polyvinyl pyrrolidone is 1:(2.5-4).
3. The mixed solution according to claim 1, characterized in that: The pH of the mixture is 5-6.5; Preferably, the pH of the mixed solution is 5.0-6.
0.
4. The mixed solution according to claim 1, characterized in that: The mass ratio of tannic acid to polyvinyl pyrrolidone is 1:3; Preferably, the molecular weight of polyvinyl pyrrolidone is 30,000-40,000.
5. The mixed solution according to any one of claims 1 to 4, characterized in that: In the mixed solution, the molar ratio of cobalt element to silver element is (6-14):
1.
6. The mixed solution according to any one of claims 1 to 4, characterized in that: The mass ratio of Ag element to tannic acid is (0.01-0.04):
1.
7. A method for preparing a mixed solution of the antibacterial spray composition according to any one of claims 1 to 6, comprising: Tannic acid and polyvinyl pyrrolidone are mixed into a first mixed solution; The first mixed solution is mixed with a soluble cobalt salt and a soluble silver salt to form a second mixed solution; Adjusting the pH of the second mixed solution to 5-9 to obtain a mixed solution of an antibacterial spray composition; Preferably, the mass ratio of tannic acid to polyvinyl pyrrolidone is 1:(2.5-4).
8. The preparation method according to claim 7, characterized in that: During the preparation of the mixture, work in dark conditions.
9. An antibacterial coating, characterized in that: The method is formed by spraying a mixed liquid of the antibacterial spray composition according to any one of claims 1 to 6 on the surface of an object; Preferably, the coating thickness is 8nm-267nm; the coating absorbance is 0.05-0.
5.
10. A method for preparing an antibacterial coating, comprising: The mixed liquid of the antibacterial spray composition according to any one of claims 1 to 6 is sprayed on the surface of an object and air-dried under natural conditions to obtain an antibacterial coating.
Citation Information
Patent Citations
Preparation method of hydrophilic antibacterial PVDF membrane
CN110898687A
Antibacterial and antiviral nano-silver colloidal solution as well as preparation method and application thereof
CN111408733A
Antiviral composition, antiviral protective film and manufacturing method thereof
CN116179002A
Process for preparing broad-spectrum antibacterial inorganic additive
CN1308866A
Antiviral composition and member having same on surface
WO2023234239A1