Heavy anti-corrosion coating and preparation method thereof
By using epoxy resin, coupling agent, dispersant and other materials in the coating, the problem of insufficient corrosion resistance of existing coatings in special industrial fields is solved, and non-toxic, low-cost, and long-term corrosion resistance protection is achieved. High adhesion and corrosion resistance of single-layer coatings.
Patent Information
- Application Number
- CN202411341685.6
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-25
- Publication Date
- 2024-12-06
AI Technical Summary
The existing coatings have insufficient corrosion resistance and insufficient adhesion, and have problems such as toxic components and high cost, and are often used in special industrial fields such as chemicals, oceans, wind and sand, and moisture. .
Using a combination of epoxy resin, coupling agent, dispersant, additive, diluent, defoaming agent, anti-aging agent and curing agent, a heavy anti-corrosion coating prepared by adding curing agent after stirring evenly, using glycidol Materials such as ether type epoxy resin, organosilane coupling agent, nano-grade titanium dioxide, polyurethane block copolymers, etc. improve the corrosion resistance and adhesion of the coating, and reduce toxicity and cost.
It realizes non-toxic, odorless, pollution-free operation, low cost, and can provide long-term and effective corrosion resistance protection under harsh environments. The single-layer coating can form a smooth and dense coating with a thickness of 300μm, and the corrosion resistance is more than 10,000 hours. , the adhesion test is level 0.
Smart Images

Figure CN119081507A_ABST
Abstract
Description
Technical Field
[0001] The invention relates to coatings and a preparation method thereof, in particular to a heavy-duty anti-corrosion coating and a preparation method thereof. Background Art
[0002] Metal equipment, devices and components used in special industrial fields such as chemical, marine, wind and sand, and humidity have high protection requirements. Existing coatings have the disadvantages of insufficient corrosion resistance, insufficient adhesion, use of toxic ingredients, high cost, and multiple times of brushing or spraying. Summary of the invention
[0003] Purpose of the invention: In order to overcome the deficiencies of the prior art, the purpose of the present invention is to provide a non-toxic, odorless and pollution-free heavy-duty anti-corrosion coating. Another purpose of the present invention is to provide a method for preparing a heavy-duty anti-corrosion coating that is simple to operate and has low cost.
[0004] Technical solution: The heavy-duty anti-corrosion coating described in the present invention includes the following substances in parts by weight: 40 to 60 parts of epoxy resin, 0.1 to 2 parts of coupling agent, 0.1 to 2 parts of dispersant, 0.5 to 10 parts of auxiliary agent, 0.5 to 2 parts of diluent, 0.1 to 2 parts of defoaming agent, 0.1 to 2 parts of antioxidant, and 10 to 20 parts of curing agent; the epoxy resin is a glycidyl ether type epoxy resin with an epoxy value of 0.41 to 0.54 eq / 100 g and a molecular weight of 500 to 2000.
[0005] Furthermore, the glycidyl ether epoxy resin is a bisphenol A epoxy resin, and its general formula is:
[0006] Furthermore, the coupling agent is organic silane.
[0007] Furthermore, the dispersant is one or more of polyurethane block copolymers and polyacrylate copolymers.
[0008] Furthermore, the auxiliary agent is nano-grade titanium dioxide with a particle size of 60 to 100 nm.
[0009] Furthermore, the diluent is one or more of ethylene oxide methyl ester, propylene oxide butyl ether, and tert-butyl acetate.
[0010] Furthermore, the defoaming agent is a silicone ether copolymer modified by grafting of polyether segments or polysiloxane segments.
[0011] Furthermore, the antioxidant is one or more of triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate and pentaerythritol propionate.
[0012] Furthermore, the curing agent is one or more of polyamides, aliphatic amines, and polyether amines.
[0013] The preparation method of a heavy-duty anti-corrosion coating described in the present invention comprises the following steps: mixing epoxy resin, coupling agent, dispersant, auxiliary agent, diluent, defoamer and antioxidant in proportion and stirring evenly; then adding curing agent and stirring evenly to obtain the heavy-duty anti-corrosion coating.
[0014] Preparation principle: The heavy-duty anti-corrosion coating of the present invention is based on epoxy resin, with the addition of polyurethane block copolymer or polyacrylate copolymer, which is beneficial to improving the toughness of the epoxy paint film; the addition of titanium dioxide is beneficial to improving the corrosion resistance, heat resistance and aging resistance of the epoxy coating; the addition of coupling agent helps to improve its adhesion; the antioxidant not only improves the service life of the coating, but also reduces the toxicity of epoxy.
[0015] Beneficial effects: Compared with the prior art, the present invention has the following significant features:.
[0016] 1. It does not contain any toxic components, the construction process is non-toxic, odorless, pollution-free, simple to operate, low cost, and can provide long-term and effective corrosion protection for metals and other materials used in harsh and harsh environments;
[0017] 2. The construction process is non-toxic, odorless and pollution-free, which can truly achieve long-term and effective protection for machines, equipment and devices used in harsh or severe environments. The coating has low cost, easy operation and is suitable for industrial production;
[0018] 3. Only one layer of brushing or spraying is needed to form a smooth and dense coating with a thickness of about 300μm. The copper accelerated acetic acid salt spray test of the coating will not show any signs of blistering, peeling, corrosion, etc. for more than 10,000 hours; the adhesion test is level 0, the cutting edge is completely smooth, and there is no shedding in the grid. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] Figure 1 is a physical picture of Example 1 of the present invention, wherein a is before the adhesion test, and b is after the adhesion test;
[0020] Figure 2 This is a physical picture of Example 2 of the present invention, wherein a is before the adhesion test, and b is after the adhesion test. DETAILED DESCRIPTION
[0021] In the following examples, the materials, reagents, etc. used can be obtained from commercial sources unless otherwise specified. The experimental methods for which specific conditions are not specified in the examples are usually carried out under conventional conditions or under conditions recommended by the manufacturer. Bisphenol A epoxy resin was purchased from Nanya Electronic Materials Co., Ltd. with an epoxy value of 0.41-0.54eq / 100g and a viscosity of 12000-15000cps / 25°C. Triethoxysilane was purchased from Shanghai McLean Biochemical Technology Co., Ltd. Polyurethane block copolymer was purchased from Shanghai McLean Biochemical Technology Co., Ltd. The auxiliary agent is 100nm titanium dioxide. The diluent is an ethylene oxide methyl ester selected from Shanghai McLean Biochemical Technology Co., Ltd. Modified silane copolymer was purchased from Shanghai McLean Biochemical Technology Co., Ltd. Triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate was purchased from Shanghai McLean Biochemical Technology Co., Ltd. Amine curing agent was purchased from Shanghai McLean Biochemical Technology Co., Ltd.
[0022] Example 1
[0023] A heavy-duty anti-corrosion coating comprises the following substances in parts by weight: 60 parts of epoxy resin, 2 parts of coupling agent, 2 parts of dispersant, 10 parts of auxiliary agent, 2 parts of diluent, 2 parts of defoamer, 2 parts of antioxidant and 20 parts of curing agent.
[0024] The epoxy resin is bisphenol A type epoxy resin, with an epoxy value of 0.41-0.47eq / 100g and a viscosity of 12000-15000cps / 25℃. The coupling agent is triethoxysilane, the dispersant is a polyurethane block copolymer, and the auxiliary agent is 100nm titanium dioxide. The diluent is an oxirane methyl ester, the defoamer is a modified silicone ether copolymer, the antioxidant is triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate, and the curing agent is an amine curing agent.
[0025] The heavy anti-corrosion coating of this embodiment is prepared by the following steps:
[0026] S1. Mix epoxy resin, coupling agent, dispersant, additive, diluent, defoamer and antioxidant according to proportion and stir evenly.
[0027] S2. Add a curing agent to the product obtained in S1, stir evenly, and obtain a heavy-duty anti-corrosion coating.
[0028] Example 2
[0029] A heavy-duty anti-corrosion coating comprises the following substances in parts by weight: 60 parts of epoxy resin, 2 parts of coupling agent, 2 parts of dispersant, 10 parts of auxiliary agent, 2 parts of diluent, 2 parts of defoamer, 2 parts of antioxidant and 20 parts of curing agent.
[0030] The epoxy value of the epoxy resin (bisphenol A glycidyl ether type epoxy resin) is 0.48-0.54eq / 100g, and the viscosity is 12000-15000cps / 25℃. The coupling agent is triethoxysilane, the dispersant is polyacrylate copolymer, and the auxiliary agent is 60nm titanium dioxide. The diluent is propylene oxide butyl ether, the defoamer is modified silicone ether copolymer, the antioxidant is pentaerythritol propionate, and the curing agent is a polyamide curing agent.
[0031] The heavy anti-corrosion coating of this embodiment is prepared by the following steps:
[0032] S1. Mix epoxy resin, coupling agent, dispersant, additive, diluent, defoamer and antioxidant according to proportion and stir evenly.
[0033] S2. Add a curing agent to the product obtained in S1, stir evenly, and obtain a heavy-duty anti-corrosion coating.
[0034] Example 3
[0035] A heavy-duty anti-corrosion coating comprises the following substances in parts by weight: 60 parts of epoxy resin, 2 parts of coupling agent, 2 parts of dispersant, 10 parts of auxiliary agent, 2 parts of diluent, 2 parts of defoamer, 2 parts of antioxidant and 20 parts of curing agent.
[0036] The epoxy resin is bisphenol A glycidyl ether type epoxy resin, with an epoxy value of 0.41-0.47eq / 100g and a viscosity of 12000-15000cps / 25°C. The coupling agent is triethoxysilane, the dispersant is polyacrylate copolymer, and the auxiliary agent is 100nm titanium dioxide. The diluent is propylene oxide butyl ether, the defoamer is a modified silicone ether copolymer, the antioxidant is triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate, and the curing agent is a fatty amine curing agent.
[0037] The heavy anti-corrosion coating of this embodiment is prepared by the following steps:
[0038] S1. Mix epoxy resin, coupling agent, dispersant, additive, diluent, defoamer and antioxidant according to proportion and stir evenly.
[0039] S2. Add a curing agent to the product obtained in S1, stir evenly, and obtain a heavy-duty anti-corrosion coating.
[0040] Example 4
[0041] The remaining specific components and preparation methods of this embodiment are the same as those of Example 1, except that the heavy anti-corrosion coating includes the following substances in parts by weight: 40 parts of epoxy resin, 0.1 parts of coupling agent, 0.1 parts of dispersant, 0.5 parts of auxiliary agent, 0.1 parts of diluent, 0.1 parts of defoaming agent, 2 parts of antioxidant, and 10 parts of curing agent.
[0042] Example 5
[0043] The remaining specific components and preparation methods of this embodiment are the same as those of Example 1, except that the heavy anti-corrosion coating includes the following substances in parts by weight: 50 parts of epoxy resin, 1 part of coupling agent, 1 part of dispersant, 5 parts of auxiliary agent, 1 part of diluent, 1 part of defoamer, 1 part of antioxidant, and 15 parts of curing agent.
[0044] Comparative Example 1 (Q235)
[0045] An uncoated low carbon steel Q235 (15mm×15mm×5mm), the specific steps are as follows:
[0046] Q235 steel with a size of 15 mm × 15 mm × 5 mm was polished to be smooth, ultrasonically cleaned in an acetone solution for 15 min, then washed with anhydrous ethanol and dried, and packaged for testing.
[0047] Comparative Example 2 (pure epoxy resin)
[0048] A preparation method of pure epoxy resin coating, the specific steps are as follows:
[0049] Mix 1 part of bisphenol A epoxy resin with 0.1 part of ethanol, stir evenly, then add 0.5 part of curing agent, stir evenly, apply on the surface of Q235 steel, cure at room temperature for 24 hours, and the dry film thickness is about 60μm. Pure epoxy resin coating is obtained.
[0050] Comparative Example 3
[0051] The remaining steps and composition of this comparative example are the same as those of Example 1, with the only difference being that the dispersant is replaced by saponified ethyl oleate, and the antioxidant is replaced by antioxidant 1010.
[0052] Performance Testing
[0053] 1. Dry film thickness
[0054] According to GB / T 13452.2-2008 / ISO 2808:2007, the thickness of the dry film after curing is tested using a thickness gauge.
[0055] 2. Salt spray test
[0056] According to GB / T 10125-2012 / ISO 9227:2006, paraffin wax and rosin were used to seal the coating edges, and appropriate amounts of glacial acetic acid and copper oxide (CuCl2·2H2O) were added to the sodium chloride salt solution. The copper ion-accelerated acetic acid rapid salt spray test (CASS test) was used to test its corrosion resistance.
[0057] 3. Adhesion Test
[0058] According to GB / T9286-2021 / ISO2409:2020, 36 grids are drawn on the coating surface, and then the grids are torn with tape to grade the coating shedding at the intersections.
[0059] Table 1 Performance of coatings in the present invention and comparative examples
[0060]
[0061] As can be seen from Table 1, the coatings of Examples 1 to 5 of the present invention are applied to Q235 steel, and only one layer of brushing or spraying is required to form a dry film coating with a thickness of about 300 μm. The surface of this coating is smooth and dense, and the copper accelerated acetic acid salt spray test will not show any signs of blistering, peeling, corrosion, etc. for more than 10,000 hours; the adhesion test is level 0, the cutting edge is completely smooth, and there is no shedding in the grid. The coating preparation method is simple, the construction process is non-toxic and tasteless, and there is no pollution, and it truly realizes long-term and effective corrosion resistance protection for machines, equipment, devices, etc. used in harsh or harsh environments.
[0062] Among the above embodiments, the best embodiment is Embodiment 1.
Claims
1. A heavy-duty anti-corrosion coating, characterized in that: The invention comprises the following substances in parts by weight: 40 to 60 parts of epoxy resin, 0.1 to 2 parts of coupling agent, 0.1 to 2 parts of dispersant, 0.5 to 10 parts of auxiliary agent, 0.5 to 2 parts of diluent, 0.1 to 2 parts of defoamer, 0.1 to 2 parts of antioxidant and 10 to 20 parts of curing agent; the epoxy resin is a glycidyl ether type epoxy resin with an epoxy value of 0.41 to 0.54 eq / 100 g and a molecular weight of 500 to 2000.
2. A heavy-duty anti-corrosion coating according to claim 1, characterized in that: The glycidyl ether epoxy resin is bisphenol A epoxy resin.
3. A heavy-duty anti-corrosion coating according to claim 1, characterized in that: The coupling agent is organic silane.
4. A heavy-duty anti-corrosion coating according to claim 1, characterized in that: The dispersant is one or more of a polyurethane block copolymer and a polyacrylate copolymer.
5. A heavy-duty anti-corrosion coating according to claim 1, characterized in that: The auxiliary agent is nano-grade titanium dioxide.
6. A heavy-duty anti-corrosion coating according to claim 1, characterized in that: The diluent is one or more of ethylene oxide methyl ester, propylene oxide butyl ether and tert-butyl acetate.
7. A heavy-duty anti-corrosion coating according to claim 1, characterized in that: The defoamer is a silicone ether copolymer obtained by grafting and modifying polyether segments or polysiloxane segments.
8. A heavy-duty anti-corrosion coating according to claim 1, characterized in that: The antioxidant is one or more of triethylene glycol ether-di(3-tert-butyl-4-hydroxy-5-methylphenyl) propionate and pentaerythritol propionate.
9. A heavy-duty anti-corrosion coating according to claim 1, characterized in that: The curing agent is one or more of polyamides, aliphatic amines and polyether amines.
10. The method for preparing a heavy-duty anti-corrosion coating according to any one of claims 1 to 9, characterized in that: The following steps are involved: The epoxy resin, coupling agent, dispersant, additive, diluent, defoamer and antioxidant are mixed in proportion and stirred evenly; then a curing agent is added and stirred evenly to obtain a heavy-duty anti-corrosion coating.
Citation Information
Patent Citations
Anti-UV epoxy resin composite coating and preparation method thereof
CN109021766A
Low-VOC epoxy primer suitable for engineering machinery coating and preparation method thereof
CN111171673A
Cited By
Pb-Mg-Si-C composite hollow sphere with high corrosion resistance and preparation method of Pb-Mg-Si-C composite hollow sphere
CN120138811A