Polyurethane composite super-hydrophobic coating and preparation method thereof
The polyurethane composite super-hydrophobic coating addresses the inefficiencies of existing coatings by using a UV/moisture dual-curing resin with modified SiO2 nanoparticles, ensuring rapid curing and enhanced durability, thus reducing energy consumption and emissions.
Patent Information
- Application Number
- CN202411288228.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-14
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-14
AI Technical Summary
Current super-hydrophobic coatings lack efficient methods for rapid curing and durability, leading to high energy consumption and VOC emissions, while failing to meet the demands for personalized and diversified products in the coatings market.
A polyurethane composite super-hydrophobic coating is developed using a UV/moisture dual-curing resin with modified SiO2 nanoparticles, incorporating organosilanes like vinyltrimethylsilane and trimethoxy(1H, 1H, 2H, 2H-heptadecafluorodecyl)silane, to create a durable and efficient coating process.
The coating achieves rapid curing, reduces VOC emissions, improves production efficiency, and enhances durability, aligning with green manufacturing practices and catering to diverse product needs.
Smart Images

Figure CN119081535A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the technical field of super hydrophobic coatings, and in particular relates to a polyurethane composite super hydrophobic coating and a preparation method thereof. Background Art
[0002] Today, technology in the fields of construction, automobiles, aerospace, etc. is developing more and more rapidly. At the same time, the current society's demand for anti-fouling and anti-corrosion materials is also increasing. The basis of anti-fouling and anti-corrosion materials is super-hydrophobic materials, which makes the research on super-hydrophobic materials more and more important.
[0003] The super-hydrophobic surface formed by the super-hydrophobic material coating also has many advantages, such as self-cleaning, oil-water separation, anti-pollution and increased material service life. Super-hydrophobic materials have both micro-nano composite structures and low surface energy chemicals, which is also a prerequisite for becoming super-hydrophobic materials. Currently, there are two main methods for making super-hydrophobic coatings: (1) constructing nano-rough structures on the surface of the material; (2) modifying the surface of the material with a coating of low surface energy substances. The contact angle of low surface energy materials will increase with the increase of surface roughness and porosity, and its hydrophobicity and self-cleaning properties will also increase accordingly.
[0004] Since super-hydrophobic coatings have excellent performance in many aspects, they are one of the research hotspots that have attracted much attention in the field of surface coatings. This application conducts further research in this direction. Summary of the invention
[0005] The present invention provides a polyurethane composite super-hydrophobic coating and a preparation method thereof. Specifically, the present invention is solved by the following technical scheme.
[0006] A polyurethane composite super-hydrophobic coating, comprising: Base layer; the base layer is a UV curable resin of HMDS modified polyurethane acrylate; The modified SiO2 nanoparticle layer is formed by spraying on the substrate layer and then curing with UV light. The modified SiO2 nanoparticles in the modified SiO2 nanoparticle layer are SiO2 nanoparticles modified with organic silane.
[0007] Preferably, the organosilane is one or more of vinyltrimethylsilane, 3-(isomethacryloyloxy)propyltrimethoxysilane, and trimethoxy(1H, 1H, 2H, 2H-heptadecafluorodecyl)silane.
[0008] Preferably, the weight proportion of the organosilane used as a raw material for modifying the SiO2 nanoparticles is 15.8 to 16.3 times the weight proportion of the SiO2 nanoparticles.
[0009] Preferably, the organosilane is a mixture of vinyltrimethylsilane, 3-(isomethacryloyloxy)propyltrimethoxysilane and trimethoxy(1H, 1H, 2H, 2H-heptadecafluorodecyl)silane in a weight ratio of 1:1.66-1.68:3.82-3.84.
[0010] Preferably, the weight percentage of HMDS as a raw material is 0.028 to 0.032 of the weight percentage of the polyurethane prepolymer before modification.
[0011] A method for preparing a polyurethane composite super-hydrophobic coating in the present application comprises the following steps: S10: Preparation of modified SiO2 nanoparticles: dissolve SiO2 in an organic solvent, disperse it by ultrasonication, then raise the temperature to 80°C~90°C and add organic silane to react; after the reaction, obtain the solid phase in the reaction solution, wash and dry it to obtain modified SiO2 nanoparticles; S20: Preparation of HMDS-modified PUA prepolymer (H-PUA): PTMEG is added to a reaction vessel, heated to the reaction temperature, IPDI and DABCO are added to the reaction vessel, reacted, and a polyurethane prepolymer is obtained; then HMDS is added to the reaction vessel for siloxane modification to obtain a partially siloxane-terminated polyurethane; then HEMA is added to the reaction vessel for complete end-capping to obtain an HMDS-modified PUA photoactive prepolymer, called H-PUA; S30: Preparation of modified nano-SiO2 / H-PUA composite super-hydrophobic coating: H-PUA, HDDA and TPO are mixed, heated and stirred, and the mixture is evenly mixed to obtain a UV / moisture dual-cured PUA substrate, and the UV / moisture dual-cured PUA substrate is used as the first layer of the coating, and the first layer is surface-dried under UV light irradiation; the modified SiO2 nanoparticles are dissolved in a solvent, and TPO is added to the solution. After it is evenly dispersed, a second layer is formed on the first layer that has not dried completely, and then UV light is irradiated; after drying, a modified nano-SiO2 / H-PUA composite super-hydrophobic coating is obtained.
[0012] Furthermore, in step S10: the organic solvent is toluene, the weight ratio of SiO2 to toluene is 1:180-220; the weight ratio of SiO2 to organic silane is 1:15.8-16.3; and the drying temperature is lower than 70°C.
[0013] Furthermore, in step S10, the organosilane is a mixture of vinyltrimethylsilane, 3-(isomethacryloyloxy)propyltrimethoxysilane, and trimethoxy(1H, 1H, 2H, 2H-heptadecafluorodecyl)silane in a weight ratio of 1:1.66-1.68:3.82-3.84.
[0014] Furthermore, in step S20, the weight ratio of PTMEG, IPDI, DABCO, and HMDS is 10: 3.7±0.1: 0.015±0.001: 0.46±0.01; after HEMA is capped, the reaction progress is detected by hydrochloric acid-di-n-butylamine titration method, and the reaction is stopped when the isocyanate group is completely consumed.
[0015] Furthermore, in step S30: the weight ratio of H-PUA, HDDA, and TPO is 1:1:0.06; the weight ratio of modified SiO2 nanoparticles and TPO is 147±3:100; and the drying temperature is lower than 70°C.
[0016] Compared with the prior art, the present invention has the following beneficial effects: In the present application, the UV / moisture dual-curing resin used can achieve rapid curing of the coating under the dual effects of ultraviolet light and moisture, and has excellent hardness and durability after curing, and can also effectively reduce VOCs emissions, which not only improves production efficiency, reduces coating costs, but also reduces energy consumption, conforms to the green and efficient development trend of modern manufacturing industry, and can meet the needs of personalized and diversified products in the coatings market. BRIEF DESCRIPTION OF THE DRAWINGS
[0017] Figure 1 Schematic diagram of the synthesis route of the modified SiO2 nanoparticles in the present invention.
[0018] Figure 2 Schematic diagram of the synthesis route of H-PUA in the present invention.
[0019] Figure 3 Middle: a is the FE-SEM image before SiO2 nanoparticle modification; b is the FE-SEM image after SiO2 nanoparticle modification; c is the FE-SEM image of the composite superhydrophobic coating with modified SiO2 nanoparticles; d is the FE-SEM image of the composite superhydrophobic coating without modified SiO2 nanoparticles.
[0020] Figure 4 Middle: a is the infrared spectrum of SiO2 nanoparticles; b is the infrared spectrum of H-PUA. DETAILED DESCRIPTION
[0021] The present invention is further described in detail below in conjunction with the accompanying drawings and specific embodiments.
[0022] In the following embodiments, the described embodiments are exemplary and are only used to explain the present invention, and should not be construed as limiting the present invention.
[0023] Reference Figure 1 and attached Figure 2 , the following is the preparation method of the polyurethane composite super-hydrophobic coating in this application.
[0024] (1) Preparation of modified SiO2 nanoparticles: 0.2 g SiO2 was dissolved in 40 g toluene and ultrasonically dispersed for 30 min. The solution was then transferred to a 250 mL four-necked flask. The temperature of the flask was raised to 85 °C, and 0.494 g vinyltrimethylsilane (VTMS), 0.828 g 3-(isobutyleneoxy)propyltrimethoxysilane (KH570) and 1.894 g trimethoxy(1H,1H,2H,2H-heptadecafluorodecyl)silane (KH1731) were added in sequence. The reaction was continued for 5 h. After the reaction was completed, the solid phase was obtained by centrifugation at 8000 rpm / min, and washed three times with ethanol. Then, the modified SiO2 nanoparticles were obtained after drying at 60 °C for 24 h.
[0025] (2) Preparation of HMDS-modified PUA prepolymer (H-PUA): 10g PTMEG was placed in a vacuum oven at 120℃ for drying and dehydration, and then transferred into a four-necked flask. After the temperature was raised to 45±2℃, 3.731g IPDI and 0.015g DABCO were added. Under this condition, the polyurethane prepolymer was obtained after constant temperature reaction for 2 hours. Then the temperature was raised to 60±2℃ and 0.465g HMDS was added for siloxane modification. The reaction was kept at constant temperature for 3 hours, and a partially siloxane-terminated polyurethane was obtained. Finally, 1.301g HEMA was added for complete end-capping. After end-capping, the reaction progress was detected by hydrochloric acid-di-n-butylamine titration method. If the reaction was stopped when the isocyanate group was completely consumed, the HMDS-modified PUA photoactive prepolymer (H-PUA) was obtained.
[0026] (3) Preparation of modified nano-SiO2 / H-PUA composite super-hydrophobic coating: Take 3 g of H-PUA, add 3 g of HDDA and 0.18 g of TPO, heat and stir, mix evenly to obtain a UV / moisture dual-cured PUA substrate. After defoaming, apply a layer on the surface of the glass slide by scraping, and then quickly dry under UV light; then dissolve 0.147 g of modified SiO2 nanoparticles in 2 g of ethanol and add 0.1 g of TPO for ultrasonic dispersion for 10 minutes. After it is completely dispersed, spray it evenly on the H-PUA coating that has not dried completely, and then irradiate it with UV light. Finally, put the glass slide in a 60°C oven and dry it for 12 h to obtain a modified nano-SiO2 / polyurethane composite super hydrophobic coating.
[0027] (4) Isocyanate content test: Add 5 ml of anhydrous toluene to a conical flask containing 0.5-1.0 g of sample, then add 10 mL of 0.1 mol / L di-n-butylamine-toluene solution, shake well to react, then add 10 mL of isopropanol and a drop of bromophenol blue, and finally titrate with 0.5 mol / L hydrochloric acid. The end point is when the indicator color changes from blue to yellow.
[0028] In the above specific embodiments, the material proportions are all determined values. It is foreseeable that the error range of the material weight proportion is within ±0.05 times the determined range in the above embodiments, which can achieve the invention purpose of the present application; in addition, the reaction temperature, reaction time, drying temperature and other parameters in the above embodiments have an allowable error range within ±0.1 times, which can also achieve the invention purpose of the present application.
[0029] Figure 1 and Figure 2 Schematic diagram of the synthesis route of modified SiO2 nanospheres and H-PUA. Figure 3 FE-SEM images of the composite superhydrophobic coating before (a) and after (b) SiO2 nanoparticle modification and the corresponding states.
[0030] Specifically, Figure 3 The unmodified SiO2 nanoparticles in a present a smooth spherical structure, while Figure 3 In b, there are organic substances attached to the surface of the spherical SiO2 nanoparticles, and the surface roughness increases; Figure 3 c It can be seen that the surface of the unmodified SiO2 nanoparticles is very flat. Due to the lack of surface roughness and low surface energy substances modifying its surface, the coating exhibits hydrophilic properties. Figure 3 In d, nano-rough structures are clearly seen where the modified SiO2 nanoparticles are present, and the SiO2 nanoparticles are modified using low-surface-weight materials such as organic fluorides, which makes the resulting coating have excellent superhydrophobic properties.
[0031] Figure 4 Infrared spectra of (a) SiO2 nanospheres and (b) H-PUA. The images were measured at room temperature of 23 °C and humidity of 33%. The samples were in powder form.
[0032] Specifically, Figure 4 The infrared spectrum of modified SiO2 nanoparticles of a shows: 3430 cm -1 It is the characteristic peak of hydroxyl group OH, 2970 cm -1 The -CH3 stretching vibration peak is at 1634 cm -1 The peak at 1209 cm is the C=C double bond stretching vibration peak. -1 The peak at 1096 cm is the CF stretching vibration peak, the peak at 803 cm is the antisymmetric stretching vibration absorption peak of Si-O bond, and the peak at 1096 cm is the antisymmetric stretching vibration absorption peak of Si-O bond. -1 The absorption peak of the symmetrical stretching vibration of Si-O bond is 434 cm -1 The absorption peak at the center is the bending vibration absorption peak of Si-O bond, which proves the successful modification of SiO2 nanoparticles.
[0033] Figure 4 In the infrared spectrum of modified H-PUA of b, we can see: 3354 cm -1 The characteristic peak of NH stretching vibration is 1724 cm -1 The characteristic peak of C=O is 1643 cm -1 and 809 cm -1 The stretching vibration peak of C=C double bond appeared at 1100 cm -1 and 806 cm -1 The corresponding peaks are the antisymmetric stretching vibration absorption peak and the symmetric stretching vibration peak of the Si-O bond in siloxane. -1 There is no obvious -NCO characteristic peak around the center, which can prove that H-PUA modified by HMDS was successfully synthesized.
[0034] Siloxane is easily hydrolyzed to form silanol, which is easy to undergo hydrolysis and polycondensation reaction with the hydroxyl groups on the surface of inorganic nanoparticles, thereby coupling the inorganic nanoparticles with siloxane to achieve modification. Due to the oxygen inhibition effect of UV light curing, the sticky property of the surface after UV light curing is utilized to make it easier for nanoparticles to attach.
[0035] Hexamethyldisilazane (HMDS) is an important organosilicon compound that is easily hydrolyzed to form hexamethyldisiloxane, which is often used as a tackifier for the surface adhesion of photoresists and can be used to improve the adhesion performance of the material surface. At the same time, the inorganic silicon nitrogen layer formed after its hydrolysis can protect the material from the influence of humidity, oxygen and impurities. On the other hand, HMDS itself has a low surface energy, and the prepared composite coating can better achieve a superhydrophobic effect.
[0036] Based on this, the present application uses vinyltrimethylsilane (VTMS), 3-(isobutyleneoxy)propyltrimethoxysilane (KH570), and trimethoxy (1H,1H,2H,2H-heptadecafluorodecyl) silane (KH1731) to modify nano-SiO2, and uses the UV-curable resin of HMDS-modified PUA as the substrate to design a super-hydrophobic coating of polyurethane (H-PUA) coated with modified SiO2 nanoparticles on the surface. The super-hydrophobic coating constructed by this method has the characteristics of strong adhesion, not easy to fall off, and long service life.
[0037] When the HMDS content is 3% of the PUA content and the modified SiO2 nanoparticle content is 7%, the static water contact angle can reach 155.83°. At this time, the rolling angle is 0.86°, the pencil hardness is 2H, the adhesion rating is 0, and the composite coating has good physical and chemical durability.
[0038] The protection scope of the present invention includes but is not limited to the above embodiments. The protection scope of the present invention shall be based on the claims. Any replacement, deformation, and improvement of the technology that can be easily thought of by technicians in this field shall fall within the protection scope of the present invention.
Claims
1. A polyurethane composite super-hydrophobic coating, characterized in that: include: Base layer; the base layer is a UV curable resin of HMDS modified polyurethane acrylate; The modified SiO2 nanoparticle layer is formed by spraying on the substrate layer and then curing with UV light. The modified SiO2 nanoparticles in the modified SiO2 nanoparticle layer are SiO2 nanoparticles modified with organic silane.
2. A polyurethane composite super-hydrophobic coating according to claim 1, characterized in that, The organosilane is one or more of vinyltrimethylsilane, 3-(isomethacryloyloxy)propyltrimethoxysilane, and trimethoxy(1H, 1H, 2H, 2H-heptadecafluorodecyl)silane.
3. A polyurethane composite super-hydrophobic coating according to claim 2, characterized in that, The weight proportion of the organic silane used as a raw material for modifying the SiO2 nanoparticles is 15.8 to 16.3 times the weight proportion of the SiO2 nanoparticles.
4. A polyurethane composite super-hydrophobic coating according to claim 3, characterized in that, The organosilane is a mixture of vinyltrimethylsilane, 3-(isomethacryloyloxy)propyltrimethoxysilane and trimethoxy(1H, 1H, 2H, 2H-heptadecafluorodecyl)silane in a weight ratio of 1:1.66-1.68:3.82-3.
84.
5. A polyurethane composite super-hydrophobic coating according to claim 1, characterized in that, The weight percentage of HMDS as a raw material is 0.028 to 0.032 of the weight percentage of the polyurethane prepolymer before modification.
6. A method for preparing a polyurethane composite super-hydrophobic coating, characterized in that: The following steps are involved: S10: Preparation of modified SiO2 nanoparticles: Dissolve SiO2 in an organic solvent, disperse it by ultrasonic, then raise the temperature to 80℃~90℃ and add organosilane to react; After the reaction is completed, the solid phase in the reaction solution is obtained, washed and dried to obtain modified SiO2 nanoparticles; S20: Preparation of HMDS-modified PUA prepolymer (H-PUA): PTMEG is added to a reaction container, the temperature is raised to a reaction temperature, IPDI and DABCO are added to the reaction container, and reacted to obtain a polyurethane prepolymer; Then, HMDS is added to the reaction vessel for siloxane modification to obtain a partially siloxane-terminated polyurethane; Then HEMA was added to the reaction vessel for complete end-capping to obtain HMDS-modified PUA photoactive prepolymer, called H-PUA; S30: Preparation of modified nano-SiO2 / H-PUA composite super-hydrophobic coating: H-PUA, HDDA and TPO are mixed, heated and stirred, and mixed evenly to obtain a UV / moisture dual-cured PUA substrate, which is used as the first layer of the coating, and the first layer is surface-dried under UV light; The modified SiO2 nanoparticles are dissolved in a solvent, TPO is added to the solution, and after the solution is evenly dispersed, a second layer is formed on the first layer that has not been fully dried, and then UV light is used for irradiation; After drying, a modified nano-SiO2 / H-PUA composite super-hydrophobic coating was obtained.
7. The method for preparing a polyurethane composite super-hydrophobic coating according to claim 6, wherein: In step S10: The organic solvent is toluene, and the weight ratio of SiO2 to toluene is 1:180-220; The weight ratio of SiO2 to organosilane is 1:15.8~16.3; The drying temperature is below 70°C.
8. A method for preparing a polyurethane composite super-hydrophobic coating according to claim 7, characterized in that, In step S10: The organosilane is a mixture of vinyltrimethylsilane, 3-(isomethacryloyloxy)propyltrimethoxysilane and trimethoxy(1H, 1H, 2H, 2H-heptadecafluorodecyl)silane in a weight ratio of 1:1.66-1.68:3.82-3.
84.
9. The method for preparing a polyurethane composite super-hydrophobic coating according to claim 6, wherein: In step S20: The weight proportion of PTMEG, IPDI, DABCO and HMDS is: 10: 3.7±0.1: 0.015±0.001: 0.46±0.01; After HEMA capping, the reaction progress was monitored by hydrochloric acid-di-n-butylamine titration method, and the reaction was stopped when the isocyanate groups were completely consumed.
10. The method for preparing a polyurethane composite super-hydrophobic coating according to claim 6, characterized in that: In step S30: The weight ratio of PUA, HDDA and TPO is 1:1:0.06; The weight ratio of modified SiO2 nanoparticles to TPO is 147±3:100; The drying temperature is below 70°C.
Citation Information
Patent Citations
Method of preparing super-hydrophobic coating by compounding waterborne polyurethane and hydrophobic modified inorganic nanoparticles
CN109370408A
Polyurethane-based super-hydrophobic coating and preparation method thereof
CN111117472A
Flame-retardant super-hydrophobic coating and use method thereof
CN116716034A
A educational card kit for enhancing writing strength, an apparatus using it
KR1020200140986A
Cited By
Preparation method of photocuring organosilicon / SiO2 super-hydrophobic coating with micro / nano mastoid structure
CN119747185A
Preparation method of photocured organic silicon / siO2 super-hydrophobic coating with micro / nano papilla structure
CN119747185B
Preparation method and application of lignin-based super-hydrophobic coating
CN121227214A