Yellowing-resistant UV curing finish paint and preparation method thereof
Through the interaction of substances such as polyurethane acrylate, epoxy acrylate, combined with titanium dioxide and photoinitiator, the problems of yellowing resistance and poor flexibility of UV topcoat are solved, and the improvement of high hardness, wear resistance and alkali resistance are achieved. , expanding the scope of application.
Patent Information
- Application Number
- CN202411418448.5
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-12-06
AI Technical Summary
The existing UV topcoat has problems such as poor yellowing resistance and poor flexibility, which affects the service life and application scenarios of the paint.
Polyurethane acrylate, epoxy acrylate, terminal diacrylate and other substances interact with each other, combining titanium dioxide, photoinitiators and amine substances, improve the crosslinking structure and yellowing resistance of the coating through specific preparation methods, and Add wetting dispersants, defoaming agents and leveling agents to enhance the performance of the coating.
It improves the hardness, wear resistance and alkali resistance of the topcoat, enhances the yellowing and water resistance of the paint, and expands the application prospects for matching with different primers.
Smart Images

Figure BDA0005080085550000121
Abstract
Description
Technical Field
[0001] The invention relates to the technical field of coatings, and in particular to a yellowing-resistant UV-curing topcoat and a preparation method thereof. Background Art
[0002] UV coatings refer to coatings that are cured by UV radiation, and their solid content can be as high as 100%. The basic components of UV coatings include active diluents, oligomers, photoinitiators (transmitting the energy of ultraviolet photons to quickly initiate the cross-linking polymerization of monomers and oligomers), and additives (such as leveling agents, defoamers, substrate lubricants, matting agents, dispersants, stabilizers, surface slip agents, etc.). Compared with general solvent-based coatings, UV coatings cure faster and cure at room temperature. Because they do not require heating and drying, they can save 75% to 90% of energy during construction compared to conventional heat-dried coatings.
[0003] However, current UV topcoats have problems such as poor yellowing resistance and poor flexibility, which affect the service life and application scenarios of the coating and reduce its scope of use.
[0004] Therefore, there is an urgent need to provide a yellowing-resistant UV-curing topcoat and a preparation method thereof. Summary of the invention
[0005] In order to solve the above technical problems, the present invention provides a yellowing-resistant UV curing topcoat, and the raw materials for preparation include, by weight:
[0006] Polyurethane acrylate 20-50 parts;
[0007] Epoxy acrylate 10-30 parts;
[0008] 10-30 parts of terminal diacrylate;
[0009] Wetting and dispersing agent 0.3-2 parts;
[0010] 10-30 parts of titanium dioxide;
[0011] 1-3 parts of photoinitiator;
[0012] 3-5 parts of amine substances.
[0013] Preferably, calculated by weight, the preparation raw materials include:
[0014] Polyurethane acrylate 30 parts;
[0015] Epoxy acrylate 20 parts;
[0016] 20 parts of terminal diacrylates;
[0017] 1 part of wetting and dispersing agent;
[0018] 20 parts of titanium dioxide;
[0019] 2 parts of photoinitiator;
[0020] 4 parts of amine substances.
[0021] The preparation method of polyurethane acrylate comprises the following steps: adding polypropylene glycol and aliphatic diisocyanate into a reaction kettle, and then heating to 75-95° C. for reaction. When the NCO content is lower than 10%, adding acrylate substances dropwise into the reaction kettle, and continuing the reaction until the NCO content is lower than 0.5%, and then stopping the reaction to obtain polyurethane acrylate.
[0022] Preferably, the preparation method of polyurethane acrylate comprises the following steps: adding polypropylene glycol and aliphatic diisocyanate into a reaction kettle, and then heating to 75-95° C. for reaction. When the NCO (isocyanate group) content is less than 10%, 6-(4-hydroxyphenoxy)hexyl acrylate (CAS: 161841-12-9) is added dropwise into the reaction kettle, and the reaction is continued until the NCO content is less than 0.5%, and the reaction is stopped to obtain polyurethane acrylate.
[0023] The polypropylene glycol has a hydroxyl value of 102-125 mgKOH / g, a molecular weight of 900-1100, a specification of PPG-1000, and is produced by Jiangsu Dena Chemical Co., Ltd.
[0024] The aliphatic diisocyanate is selected from at least one of trimethylhexamethylene diisocyanate, butane-1,4-diisocyanate, and 1,6-hexamethylene diisocyanate; preferably, the aliphatic diisocyanate is selected from trimethylhexamethylene diisocyanate and butane-1,4-diisocyanate; the molar ratio of trimethylhexamethylene diisocyanate to butane-1,4-diisocyanate is 1:1.
[0025] The molar ratio of the polypropylene glycol to the aliphatic diisocyanate is 1:1-3; preferably, the molar ratio of the polypropylene glycol to the aliphatic diisocyanate is 1:2.
[0026] The molar ratio of the polypropylene glycol to 6-(4-hydroxyphenoxy)hexyl acrylate is 1:1-3; preferably, the molar ratio of the polypropylene glycol to 6-(4-hydroxyphenoxy)hexyl acrylate is 1:2.
[0027] The method for determining the content of the isocyanate group may be a method known in the art, such as the ASTM D-2572 method.
[0028] The present application adopts trimethylhexamethylene diisocyanate and butane-1,4-diisocyanate to prepare polyurethane acrylate with strong yellowing resistance. At the same time, by adding 6-(4-hydroxyphenoxy)hexyl acrylate, the structure of polyurethane acrylate is adjusted, thereby improving the yellowing resistance and water resistance of the coating.
[0029] The epoxy acrylate is bisphenol A epoxy diacrylate, CAS number: 89297-97-2.
[0030] The terminal diacrylate is selected from at least one of propoxylated neopentyl glycol diacrylate, dipropylene glycol diacrylate, and tripropylene glycol diacrylate; preferably, the terminal diacrylate is selected from propoxylated neopentyl glycol diacrylate and dipropylene glycol diacrylate; further preferably, the weight ratio of propoxylated neopentyl glycol diacrylate (CAS: 84170-74-1) to dipropylene glycol diacrylate is 1:3. In the present application, by using propoxylated neopentyl glycol diacrylate (CAS: 84170-74-1) and dipropylene glycol diacrylate, in addition to increasing the reaction activity, the cross-linking structure of the coating is also improved.
[0031] The wetting and dispersing agent is a high molecular weight styrene-acrylic acid modified polymer, the model is dispersant 5027H, and the manufacturer is Huayue Fine Chemicals (Kunshan) Co., Ltd.
[0032] The titanium dioxide is rutile titanium dioxide produced by the sulfate process and subjected to inorganic surface treatment with zirconium oxide and aluminum oxide.
[0033] The photoinitiator is selected from one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxy-cyclohexyl-phenyl ketone, benzophenone, and benzoin dimethyl ether; preferably, the photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone.
[0034] The amine substance includes at least one of polyetheramine, meta-xylene diamine, isophorone diamine, diethylenetriamine, triethylenetetramine, and tetraethylenepentamine; preferably, the amine substance is diethylenetriamine.
[0035] It also includes: 0.3-1 part of silicon dioxide; 0.1-0.5 part of defoaming agent; 0.2-0.7 part of leveling agent.
[0036] The silicon dioxide is RAD 2005 silica, manufactured by Grace, USA.
[0037] The defoamer described in this application is a commonly used organic silicon defoamer in the art, which can fully defoam during the construction process without affecting the appearance of the paint film; the manufacturers include BASF, Shin-Etsu, etc. The defoamer in this application is Shin-Etsu KSZ-108 defoamer.
[0038] The leveling agent is a polyether siloxane copolymer, and its model is TEGO Gl ide410.
[0039] The preparation method of the topcoat comprises the following steps: mixing the weight portions of polyurethane acrylate, epoxy acrylate, terminal diacrylate, titanium dioxide, amine substances, silicon dioxide, leveling agent and wetting dispersant, stirring fully, and then adding a photoinitiator and a defoamer and stirring fully to obtain the topcoat.
[0040] The curing energy of this product is 200-250mg / cm 2 .
[0041] By adopting the above technical solution, the present invention has the following beneficial effects:
[0042] 1. This application improves the cross-linking structure of the topcoat through the interaction of materials such as polyurethane acrylate, epoxy acrylate, and terminal diacrylate, thereby improving the hardness and wear resistance.
[0043] 2. The topcoat prepared in this application has excellent yellowing resistance and alkali resistance.
[0044] 3. The UV topcoat can be matched with different primers, such as PU primer, PE primer, UV primer, etc., and has a good application prospect. DETAILED DESCRIPTION
[0045] The technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.
[0046] The present invention is further explained below in conjunction with specific implementation modes.
[0047] Example 1
[0048] A yellowing-resistant UV curing topcoat, calculated by weight, comprising the following raw materials:
[0049] Polyurethane acrylate 30 parts;
[0050] Epoxy acrylate 20 parts;
[0051] 20 parts of terminal diacrylates;
[0052] 1 part of wetting and dispersing agent;
[0053] 20 parts of titanium dioxide;
[0054] 2 parts of photoinitiator;
[0055] 4 parts of amine substances;
[0056] 0.5 parts of silicon dioxide;
[0057] 0.3 parts of defoaming agent;
[0058] 0.5 parts of leveling agent.
[0059] The preparation method of polyurethane acrylate comprises the following steps: adding polypropylene glycol and aliphatic diisocyanate into a reaction kettle, and then heating to 85° C. for reaction. When the content of NCO (isocyanate group) is lower than 10%, 6-(4-hydroxyphenoxy)hexyl acrylate (CAS: 161841-12-9) is added dropwise into the reaction kettle, and the reaction is continued until the content of NCO is lower than 0.5%, and the reaction is stopped to obtain polyurethane acrylate.
[0060] The polypropylene glycol has a hydroxyl value of 102-125 mgKOH / g, a molecular weight of 900-1100, a specification of PPG-1000, and is produced by Jiangsu Dena Chemical Co., Ltd.
[0061] The aliphatic diisocyanate is selected from trimethylhexamethylene diisocyanate and butane-1,4-diisocyanate; the molar ratio of trimethylhexamethylene diisocyanate to butane-1,4-diisocyanate is 1:1.
[0062] The molar ratio of the polypropylene glycol to the aliphatic diisocyanate is 1:2.
[0063] The molar ratio of the polypropylene glycol to 6-(4-hydroxyphenoxy)hexyl acrylate is 1:2.
[0064] The epoxy acrylate is bisphenol A epoxy diacrylate, CAS number: 89297-97-2.
[0065] The terminal diacrylates are selected from propoxylated neopentyl glycol diacrylate and dipropylene glycol diacrylate; the weight ratio of propoxylated neopentyl glycol diacrylate to dipropylene glycol diacrylate is 1:3.
[0066] The wetting and dispersing agent is a high molecular weight styrene-acrylic acid modified polymer, the model is dispersant 5027H, and the manufacturer is Huayue Fine Chemicals (Kunshan) Co., Ltd.
[0067] The titanium dioxide is rutile titanium dioxide produced by the sulfuric acid process and subjected to inorganic surface treatment with zirconium oxide and aluminum oxide, the model is R-996, and the manufacturer is Longbai Group Co., Ltd.
[0068] The photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone.
[0069] The amine substance is diethylenetriamine.
[0070] The silicon dioxide is RAD 2005 silica, manufactured by Grace, USA.
[0071] The defoamer is Shin-Etsu KSZ-108 defoamer.
[0072] The leveling agent is a polyether siloxane copolymer, and its model is TEGO Gl ide410.
[0073] The preparation method of the topcoat comprises the following steps: mixing the weight portions of polyurethane acrylate, epoxy acrylate, terminal diacrylate, titanium dioxide, amine substances, silicon dioxide, leveling agent and wetting dispersant, stirring fully, and then adding a photoinitiator and a defoamer and stirring fully to obtain the topcoat.
[0074] Example 2
[0075] A yellowing-resistant UV curing topcoat, calculated by weight, comprising the following raw materials:
[0076] Polyurethane acrylate 50 parts;
[0077] Epoxy acrylate 30 parts;
[0078] 30 parts of terminal diacrylate;
[0079] 2 parts of wetting and dispersing agent;
[0080] 30 parts of titanium dioxide;
[0081] 3 parts of photoinitiator;
[0082] 5 parts of amine substances;
[0083] 1 part of silicon dioxide;
[0084] 0.5 parts of defoaming agent;
[0085] 0.7 parts of leveling agent.
[0086] The preparation method of polyurethane acrylate comprises the following steps: adding polypropylene glycol and aliphatic diisocyanate into a reaction kettle, and then heating to 85° C. for reaction. When the content of NCO (isocyanate group) is lower than 10%, 6-(4-hydroxyphenoxy)hexyl acrylate (CAS: 161841-12-9) is added dropwise into the reaction kettle, and the reaction is continued until the content of NCO is lower than 0.5%, and the reaction is stopped to obtain polyurethane acrylate.
[0087] The polypropylene glycol has a hydroxyl value of 102-125 mgKOH / g, a molecular weight of 900-1100, a specification of PPG-1000, and is produced by Jiangsu Dena Chemical Co., Ltd.
[0088] The aliphatic diisocyanate is selected from trimethylhexamethylene diisocyanate and butane-1,4-diisocyanate; the molar ratio of trimethylhexamethylene diisocyanate to butane-1,4-diisocyanate is 1:1.
[0089] The molar ratio of the polypropylene glycol to the aliphatic diisocyanate is 1:3.
[0090] The molar ratio of the polypropylene glycol to 6-(4-hydroxyphenoxy)hexyl acrylate is 1:3.
[0091] The epoxy acrylate is bisphenol A epoxy diacrylate, CAS number: 89297-97-2.
[0092] The terminal diacrylates are selected from propoxylated neopentyl glycol diacrylate and dipropylene glycol diacrylate; the weight ratio of propoxylated neopentyl glycol diacrylate to dipropylene glycol diacrylate is 1:3.
[0093] The wetting and dispersing agent is a high molecular weight styrene-acrylic acid modified polymer, the model is dispersant 5027H, and the manufacturer is Huayue Fine Chemicals (Kunshan) Co., Ltd.
[0094] The titanium dioxide is rutile titanium dioxide produced by the sulfuric acid process and subjected to inorganic surface treatment with zirconium oxide and aluminum oxide, the model is R-996, and the manufacturer is Longbai Group Co., Ltd.
[0095] The photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone.
[0096] The amine substance is diethylenetriamine.
[0097] The silicon dioxide is RAD 2005 silica, manufactured by Grace, USA.
[0098] The defoamer is Shin-Etsu KSZ-108 defoamer.
[0099] The leveling agent is a polyether siloxane copolymer, and its model is TEGO Gl ide410.
[0100] The preparation method of the topcoat has the same specific steps as Example 1.
[0101] Example 3
[0102] A yellowing-resistant UV curing topcoat, calculated by weight, comprising the following raw materials:
[0103] Polyurethane acrylate 20 parts;
[0104] Epoxy acrylate 10 parts;
[0105] 10 parts of terminal diacrylate;
[0106] 0.3 parts of wetting and dispersing agent;
[0107] Titanium dioxide 10 parts;
[0108] 1 part of photoinitiator;
[0109] 3 parts of amine substances;
[0110] 0.3 parts of silicon dioxide;
[0111] Defoaming agent 0.1 part;
[0112] 0.2 parts of leveling agent.
[0113] The preparation method of polyurethane acrylate comprises the following steps: adding polypropylene glycol and aliphatic diisocyanate into a reaction kettle, and then heating to 85° C. for reaction. When the content of NCO (isocyanate group) is lower than 10%, 6-(4-hydroxyphenoxy)hexyl acrylate (CAS: 161841-12-9) is added dropwise into the reaction kettle, and the reaction is continued until the content of NCO is lower than 0.5%, and the reaction is stopped to obtain polyurethane acrylate.
[0114] The polypropylene glycol has a hydroxyl value of 102-125 mgKOH / g, a molecular weight of 900-1100, a specification of PPG-1000, and is produced by Jiangsu Dena Chemical Co., Ltd.
[0115] The aliphatic diisocyanate is selected from trimethylhexamethylene diisocyanate and butane-1,4-diisocyanate; the molar ratio of trimethylhexamethylene diisocyanate to butane-1,4-diisocyanate is 1:1.
[0116] The molar ratio of the polypropylene glycol to the aliphatic diisocyanate is 1:1.
[0117] The molar ratio of the polypropylene glycol to 6-(4-hydroxyphenoxy)hexyl acrylate is 1:1.
[0118] The epoxy acrylate is bisphenol A epoxy diacrylate, CAS number: 89297-97-2.
[0119] The terminal diacrylates are selected from propoxylated neopentyl glycol diacrylate and dipropylene glycol diacrylate; the weight ratio of propoxylated neopentyl glycol diacrylate to dipropylene glycol diacrylate is 1:3.
[0120] The wetting and dispersing agent is a high molecular weight styrene-acrylic acid modified polymer, the model is dispersant 5027H, and the manufacturer is Huayue Fine Chemicals (Kunshan) Co., Ltd.
[0121] The titanium dioxide is rutile titanium dioxide produced by the sulfuric acid process and subjected to inorganic surface treatment with zirconium oxide and aluminum oxide, the model is R-996, and the manufacturer is Longbai Group Co., Ltd.
[0122] The photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone.
[0123] The amine substance is diethylenetriamine.
[0124] The silicon dioxide is RAD 2005 silica, manufactured by Grace, USA.
[0125] The defoamer is Shin-Etsu KSZ-108 defoamer.
[0126] The leveling agent is a polyether siloxane copolymer, and its model is TEGO Gl ide410.
[0127] The preparation method of the topcoat has the same specific steps as Example 1.
[0128] Comparative Example 1
[0129] A yellowing-resistant UV curing topcoat, calculated by weight, comprising the following raw materials:
[0130] Polyurethane acrylate 30 parts;
[0131] Epoxy acrylate 20 parts;
[0132] 20 parts of terminal diacrylates;
[0133] 1 part of wetting and dispersing agent;
[0134] 20 parts of titanium dioxide;
[0135] 2 parts of photoinitiator;
[0136] 4 parts of amine substances;
[0137] 0.5 parts of silicon dioxide;
[0138] 0.3 parts of defoaming agent;
[0139] 0.5 parts of leveling agent.
[0140] The preparation method of polyurethane acrylate comprises the following steps: adding polypropylene glycol and aliphatic diisocyanate into a reaction kettle, and then heating to 85° C. for reaction. When the content of NCO (isocyanate group) is lower than 10%, 6-(4-hydroxyphenoxy)hexyl acrylate (CAS: 161841-12-9) is added dropwise into the reaction kettle, and the reaction is continued until the content of NCO is lower than 0.5%, and the reaction is stopped to obtain polyurethane acrylate.
[0141] The aliphatic diisocyanate is selected from trimethylhexamethylene diisocyanate.
[0142] The polypropylene glycol has a hydroxyl value of 102-125 mgKOH / g, a molecular weight of 900-1100, a specification of PPG-1000, and is produced by Jiangsu Dena Chemical Co., Ltd.
[0143] The molar ratio of the polypropylene glycol to the aliphatic diisocyanate is 1:2.
[0144] The molar ratio of the polypropylene glycol to 6-(4-hydroxyphenoxy)hexyl acrylate is 1:2.
[0145] The epoxy acrylate is bisphenol A epoxy diacrylate, CAS number: 89297-97-2.
[0146] The terminal diacrylates are selected from propoxylated neopentyl glycol diacrylate and dipropylene glycol diacrylate; the weight ratio of propoxylated neopentyl glycol diacrylate to dipropylene glycol diacrylate is 1:3.
[0147] The wetting and dispersing agent is a high molecular weight styrene-acrylic acid modified polymer, the model is dispersant 5027H, and the manufacturer is Huayue Fine Chemicals (Kunshan) Co., Ltd.
[0148] The titanium dioxide is rutile titanium dioxide produced by the sulfuric acid process and subjected to inorganic surface treatment with zirconium oxide and aluminum oxide, the model is R-996, and the manufacturer is Longbai Group Co., Ltd.
[0149] The photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone.
[0150] The amine substance is diethylenetriamine.
[0151] The silicon dioxide is RAD 2005 silica, manufactured by Grace, USA.
[0152] The defoamer is Shin-Etsu KSZ-108 defoamer.
[0153] The leveling agent is a polyether siloxane copolymer, and its model is TEGO Gl ide410.
[0154] The preparation method of the topcoat comprises the following steps: mixing the weight portions of polyurethane acrylate, epoxy acrylate, terminal diacrylate, titanium dioxide, amine substances, silicon dioxide, leveling agent and wetting dispersant, stirring fully, and then adding a photoinitiator and a defoamer and stirring fully to obtain the topcoat.
[0155] Comparative Example 2
[0156] A yellowing-resistant UV-curing topcoat, the specific implementation method is the same as that of Example 1, except that:
[0157] Calculated by weight, the raw materials for preparation include:
[0158] Polyurethane acrylate 30 parts;
[0159] Epoxy acrylate 20 parts;
[0160] 20 parts of terminal diacrylates;
[0161] 1 part of wetting and dispersing agent;
[0162] 20 parts of titanium dioxide;
[0163] 2 parts of photoinitiator;
[0164] 4 parts of amine substances;
[0165] 0.5 parts of silicon dioxide;
[0166] 0.3 parts of defoaming agent;
[0167] 0.5 parts of leveling agent.
[0168] The preparation method of polyurethane acrylate comprises the following steps: adding polypropylene glycol and aliphatic diisocyanate into a reaction kettle, and then heating to 85° C. for reaction. When the content of NCO (isocyanate group) is lower than 10%, 6-(4-hydroxyphenoxy)hexyl acrylate (CAS: 161841-12-9) is added dropwise into the reaction kettle, and the reaction is continued until the content of NCO is lower than 0.5%, and the reaction is stopped to obtain polyurethane acrylate.
[0169] The aliphatic diisocyanate is replaced by trimethylhexamethylene diisocyanate and p-phenylene diisocyanate; the molar ratio of trimethylhexamethylene diisocyanate to p-phenylene diisocyanate is 1:1.
[0170] The polypropylene glycol has a hydroxyl value of 102-125 mgKOH / g, a molecular weight of 900-1100, a specification of PPG-1000, and is produced by Jiangsu Dena Chemical Co., Ltd.
[0171] The molar ratio of the polypropylene glycol to the aliphatic diisocyanate is 1:2.
[0172] The molar ratio of the polypropylene glycol to 6-(4-hydroxyphenoxy)hexyl acrylate is 1:2.
[0173] The epoxy acrylate is bisphenol A epoxy diacrylate, CAS number: 89297-97-2.
[0174] The terminal diacrylates are selected from propoxylated neopentyl glycol diacrylate and dipropylene glycol diacrylate; the weight ratio of propoxylated neopentyl glycol diacrylate to dipropylene glycol diacrylate is 1:3.
[0175] The wetting and dispersing agent is a high molecular weight styrene-acrylic acid modified polymer, the model is dispersant 5027H, and the manufacturer is Huayue Fine Chemicals (Kunshan) Co., Ltd.
[0176] The titanium dioxide is rutile titanium dioxide produced by the sulfuric acid process and subjected to inorganic surface treatment with zirconium oxide and aluminum oxide, the model is R-996, and the manufacturer is Longbai Group Co., Ltd.
[0177] The photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone.
[0178] The amine substance is diethylenetriamine.
[0179] The silicon dioxide is RAD 2005 silica, manufactured by Grace, USA.
[0180] The defoamer is Shin-Etsu KSZ-108 defoamer.
[0181] The leveling agent is a polyether siloxane copolymer, and its model is TEGO Gl ide410.
[0182] The preparation method of the topcoat comprises the following steps: mixing the weight portions of polyurethane acrylate, epoxy acrylate, terminal diacrylate, titanium dioxide, amine substances, silicon dioxide, leveling agent and wetting dispersant, stirring fully, and then adding a photoinitiator and a defoamer and stirring fully to obtain the topcoat.
[0183] Comparative Example 3
[0184] A yellowing-resistant UV-curing topcoat, the specific implementation method is the same as that of Example 1, except that:
[0185] Calculated by weight, the raw materials for preparation include:
[0186] Polyurethane acrylate 30 parts;
[0187] Epoxy acrylate 20 parts;
[0188] 20 parts of terminal diacrylates;
[0189] 1 part of wetting and dispersing agent;
[0190] 20 parts of titanium dioxide;
[0191] 2 parts of photoinitiator;
[0192] 4 parts of amine substances;
[0193] 0.5 parts of silicon dioxide;
[0194] 0.3 parts of defoaming agent;
[0195] 0.5 parts of leveling agent.
[0196] The preparation method of polyurethane acrylate comprises the following steps: adding polypropylene glycol and aliphatic diisocyanate into a reaction kettle, and then heating to 85° C. for reaction. When the NCO (isocyanate group) content is lower than 10%, adding 2-hydroxyethyl acrylate dropwise into the reaction kettle, and continuing the reaction until the NCO content is lower than 0.5%, and then stopping the reaction to obtain polyurethane acrylate.
[0197] The polypropylene glycol has a hydroxyl value of 102-125 mgKOH / g, a molecular weight of 900-1100, a specification of PPG-1000, and is produced by Jiangsu Dena Chemical Co., Ltd.
[0198] The aliphatic diisocyanate is selected from trimethylhexamethylene diisocyanate and butane-1,4-diisocyanate; the molar ratio of trimethylhexamethylene diisocyanate to butane-1,4-diisocyanate is 1:1.
[0199] The molar ratio of the polypropylene glycol to the aliphatic diisocyanate is 1:2.
[0200] The molar ratio of the polypropylene glycol to 2-hydroxyethyl acrylate is 1:2.
[0201] The epoxy acrylate is bisphenol A epoxy diacrylate, CAS number: 89297-97-2.
[0202] The terminal diacrylates are selected from propoxylated neopentyl glycol diacrylate and dipropylene glycol diacrylate; the weight ratio of propoxylated neopentyl glycol diacrylate to dipropylene glycol diacrylate is 1:3.
[0203] The wetting and dispersing agent is a high molecular weight styrene-acrylic acid modified polymer, the model is dispersant 5027H, and the manufacturer is Huayue Fine Chemicals (Kunshan) Co., Ltd.
[0204] The titanium dioxide is rutile titanium dioxide produced by the sulfuric acid process and subjected to inorganic surface treatment with zirconium oxide and aluminum oxide, the model is R-996, and the manufacturer is Longbai Group Co., Ltd.
[0205] The photoinitiator is 2-hydroxy-2-methyl-1-phenyl-1-propanone.
[0206] The amine substance is diethylenetriamine.
[0207] The silicon dioxide is RAD 2005 silica, manufactured by Grace, USA.
[0208] The defoamer is Shin-Etsu KSZ-108 defoamer.
[0209] The leveling agent is a polyether siloxane copolymer, and its model is TEGO Gl ide410.
[0210] The preparation method of the topcoat comprises the following steps: mixing the weight portions of polyurethane acrylate, epoxy acrylate, terminal diacrylate, titanium dioxide, amine substances, silicon dioxide, leveling agent and wetting dispersant, stirring fully, and then adding a photoinitiator and a defoamer and stirring fully to obtain the topcoat.
[0211] Performance Testing
[0212] The topcoats prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were cured and then subjected to performance tests.
[0213] Yellowing resistance: reference standard GB / 23997-2009.
[0214] Alkali resistance: refer to standard GB / 23997-2009, use 50g / L sodium carbonate solution, test for 2h.
[0215] Flexibility: Reference standard GB / T1731-93.
[0216] Water resistance: Reference standard GB / T1731-93.
[0217] Table 1 Performance test
[0218]
[0219] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention, rather than to limit it. Although the present invention has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or replace some or all of the technical features therein with equivalents. However, these modifications or replacements do not cause the essence of the corresponding technical solutions to deviate from the scope of the technical solutions of the embodiments of the present invention.
Claims
1. A yellowing-resistant UV-curing topcoat, characterized in that: Calculated by weight, the raw materials for preparation include: Polyurethane acrylate 20-50 parts; Epoxy acrylate 10-30 parts; 10-30 parts of terminal diacrylates; Wetting and dispersing agent 0.3-2 parts; 10-30 parts of titanium dioxide; 1-3 parts of photoinitiator; 3-5 parts of amine substances.
2. The topcoat as claimed in claim 1, characterized in that Calculated by weight, the preparation raw materials include: Polyurethane acrylate 30 parts; Epoxy acrylate 20 parts; 20 parts of terminal diacrylates; 1 part of wetting and dispersing agent; 20 parts of titanium dioxide; 2 parts of photoinitiator; 4 parts of amine substances.
3. The topcoat according to claim 1, characterized in that The preparation method of polyurethane acrylate comprises the following steps: adding polypropylene glycol and aliphatic diisocyanate into a reaction kettle, then heating to 75-95°C for reaction, when the NCO content is lower than 10%, dripping acrylate substances into the reaction kettle, continuing the reaction until the NCO content is lower than 0.5%, stopping the reaction, and obtaining polyurethane acrylate.
4. The topcoat as claimed in claim 3, characterized in that The molar ratio of the polypropylene glycol to the aliphatic diisocyanate is 1:1-3.
5. The topcoat as claimed in claim 3, characterized in that The aliphatic diisocyanate is at least one selected from trimethylhexamethylene diisocyanate, butane-1,4-diisocyanate, and hexamethylene diisocyanate.
6. The topcoat according to claim 1, characterized in that The terminal diacrylate is selected from at least one of propoxylated neopentyl glycol diacrylate, dipropylene glycol diacrylate and tripropylene glycol diacrylate.
7. The topcoat according to claim 1, characterized in that The photoinitiator is selected from one or more of 2-hydroxy-2-methyl-1-phenyl-1-propanone, 1-hydroxy-cyclohexyl-phenyl ketone, benzophenone, and benzoin dimethyl ether.
8. The topcoat according to claim 1, characterized in that The raw materials for preparing the topcoat also include 0.3-1 part of silicon dioxide, 0.1-0.5 part of defoaming agent, and 0.2-0.7 part of leveling agent.
9. The topcoat as claimed in claim 8, characterized in that The leveling agent is a polyether siloxane copolymer.
10. A method for preparing a topcoat according to any one of claims 1 to 9, characterized in that: The method comprises the following steps: mixing the polyurethane acrylate, epoxy acrylate, terminal diacrylate, titanium dioxide, amine substances, silicon dioxide, leveling agent and wetting dispersant in the above mentioned weight parts and stirring them fully, and then adding a photoinitiator and a defoamer and stirring them fully to obtain the product.
Citation Information
Patent Citations
Novel odorless high-weather-resistance LED-UV photocuring white finish paint and production mode thereof
CN112760017A
Matt skin-touch finish paint and use method thereof
CN117210120A