Coating as well as preparation method and application thereof

Through the combination of methylphenyl modification and epoxy modified silicone resin, combined with methacryloyloxypropyl cage silsesquioxane modification technology, the adhesion of high-temperature resistant coatings under thick coatings is solved. The problem of high temperature resistance performance achieves the effect of high temperature not easy to crack, and simplifies construction operations, avoiding the need to use high temperature resistant fillers.

CN119081549APending Publication Date: 2024-12-06GUANGDONG DAER NOVEL MATERIALS CO LTD
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411355594.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-27
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

When the coating thickness of existing high-temperature resistant coatings are thicker, it is difficult to maintain good adhesion and high-temperature resistant performance, and high-temperature resistant fillers such as aluminum powder and glass powder are required, resulting in complex construction operations and high risk of high-temperature cracking.

Method used

The vinyl-containing methylphenyl-modified silicone resin is modified by methacryloyloxypropyl cage-type silsesquioxane. It can reduce the degradation caused by Si-OH and terminal hydroxyl groups, form a tight mesh structure, avoid the coating cracking at high temperatures, and do not need to add high-temperature resistant fillers.

Benefits of technology

In the case of thick coating thickness, the coating has good high temperature resistance and adhesion, which is not easy to crack at high temperatures, simplifies construction operations, and can be made into varnish without the need for additional high temperature resistant fillers.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure BDA0005063518680000021
    Figure BDA0005063518680000021
  • Figure BDA0005063518680000091
    Figure BDA0005063518680000091
  • Figure BDA0005063518680000092
    Figure BDA0005063518680000092
Patent Text Reader

Abstract

The invention belongs to the technical field of coatings, and particularly relates to a coating as well as a preparation method and application thereof. The coating comprises methyl phenyl modified organic silicon resin and epoxy modified organic silicon resin. The methyl phenyl modified organic silicon resin is obtained by modifying methyl phenyl silicon resin containing vinyl by adopting methacryloyloxypropyl polyhedral oligomeric silsesquioxane. Methylacryloyloxypropyl polyhedral oligomeric silsesquioxane is adopted to modify methyl phenyl silicon resin containing vinyl, through compounding of methyl phenyl modified organic silicon resin and epoxy modified organic silicon resin, through the combined action of the methyl phenyl modified organic silicon resin and the epoxy modified organic silicon resin, the coating can be prepared into a high-film-thickness coating, and under the condition that the coating is thick, the high-film-thickness coating can be prepared into a high-film-thickness coating. The coating still has good high temperature resistance, such as good adhesive force, and is not easy to crack at high temperature, and the coating does not crack after an impact test, so that the construction operation is convenient. Meanwhile, the coating has good high-temperature resistance, and high-temperature-resistant filler is not required to be added, so that the coating can be made into varnish.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of coatings, and in particular relates to a coating and a preparation method and application thereof. Background Art

[0002] High temperature resistant coatings are widely used in various high temperature places, such as steel chimneys, high temperature pipelines, high temperature furnaces, oil cracking devices, and the inner and outer surfaces of military equipment, etc., to solve the thermal oxidation corrosion of metals at high temperatures, ensure the safe operation of equipment and extend its service life.

[0003] Silicone varnish is a main type of high temperature resistant coating. It is usually based on silicone resin or modified silicone resin, with accelerator, wetting agent and defoamer, and xylene to prepare single-component or two-component silicone high temperature resistant coating to meet the needs of different fields. Silicone resin has good heat resistance. It is prepared into silicone high temperature resistant coating with methyl silicone resin and methylphenyl silicone resin. It is usually necessary to add high temperature resistant fillers such as aluminum powder, glass powder, mica powder, etc. to improve the high temperature resistance, but it cannot be made into varnish. Although the addition of the above substances can improve the high temperature resistance, the adhesion of the paint film can only be guaranteed when the film thickness is low, which will lead to high construction operation requirements and a greater risk of high temperature cracking.

[0004] Therefore, there is an urgent need to provide a coating that still has good high temperature resistance, such as good adhesion, and is not prone to cracking at high temperatures even when the coating thickness is relatively thick. Summary of the invention

[0005] The present invention aims to solve one or more technical problems existing in the above-mentioned prior art, and at least provide a beneficial choice or create conditions. Specifically, the present invention provides a coating, which has good high temperature resistance, such as good adhesion, and is not easy to crack at high temperature, even when the coating thickness is relatively thick, thereby facilitating construction operations. At the same time, since there is no need to add high temperature resistant fillers, such as aluminum powder, glass powder, mica powder, etc., the coating of the present invention can be made into varnish.

[0006] The inventive concept of the present invention: The coating of the present invention includes methylphenyl modified silicone resin and epoxy modified silicone resin; the methylphenyl modified silicone resin is obtained by modifying the vinyl-containing methylphenyl silicone resin with methacryloxypropyl cage silsesquioxane. The vinyl-containing methylphenyl silicone resin of the present invention can greatly reduce the number of terminal hydroxyl groups, and by modifying the vinyl-containing methylphenyl silicone resin with methacryloxypropyl cage silsesquioxane, the "unbuttoning" type degradation caused by Si-OH of the silicone resin can be reduced or even avoided, and the "unbuttoning" type degradation caused by the terminal hydroxyl groups can be reduced or even avoided, thereby improving the heat resistance of the silicone resin. After the coating is cured, a tight network structure is generated, and even under thermal stress, the cured coating can prevent cracks from forming. The present invention uses a compound of methylphenyl modified silicone resin and epoxy modified silicone resin, and the two work together to make the coating be prepared into a high film thickness coating. When the coating thickness is relatively thick, it still has good high temperature resistance, such as good adhesion, and is not easy to crack at high temperature, thereby facilitating construction operations. At the same time, since the coating of the present invention has good high temperature resistance, it is not necessary to add high temperature resistant fillers such as aluminum powder, glass powder, mica powder, etc., and can be made into varnish.

[0007] Therefore, a first aspect of the present invention provides a coating.

[0008] Specifically, the coating includes methylphenyl modified silicone resin and epoxy modified silicone resin;

[0009] The methylphenyl modified silicone resin is obtained by modifying a vinyl-containing methylphenyl silicone resin with methacryloxypropyl cage-type silsesquioxane.

[0010] Preferably, the structural formula of the methylphenyl modified silicone resin is:

[0011]

[0012] Wherein, the R1 is selected from any one of methyl and phenyl, the R2 is selected from any one of methyl and phenyl, and R1 and R2 are different; and n is 4000-6000.

[0013] Preferably, the methylphenyl-modified silicone resin is a methacryloxyphenyl silicone resin.

[0014] Preferably, the epoxy-modified silicone resin is obtained by modifying silicone oligomers with epoxy resin.

[0015] Preferably, the epoxy-modified silicone resin includes Japan Shin-Etsu ES-1001N.

[0016] Preferably, the coating further comprises at least one of an auxiliary agent and a solvent.

[0017] Preferably, the auxiliary agent includes at least one of a promoter, a wetting agent and a defoaming agent.

[0018] Preferably, the coating further comprises an accelerator, a wetting agent, a defoamer and a solvent; and in terms of mass percentage, the coating comprises 36-45% methylphenyl-modified silicone resin, 36-45% epoxy-modified silicone resin, 0.5-3.3% accelerator, 0.2-0.55% wetting agent, 0.2-0.55% defoamer and 5.6-27.1% solvent.

[0019] Further preferably, the coating also includes an accelerator, a wetting agent, a defoamer, and a solvent; and in terms of mass percentage, the coating includes 40-45% methylphenyl-modified silicone resin, 40-45% epoxy-modified silicone resin, 0.5-3% accelerator, 0.2-0.5% wetting agent, 0.2-0.5% defoamer, and 6-19.1% solvent.

[0020] Preferably, the accelerator comprises an organic accelerator.

[0021] More preferably, the accelerator includes at least one of zinc isooctanoate, cobalt isooctanoate, and tetrabutyl titanate.

[0022] Preferably, the wetting agent includes at least one of an organic silicon compound and an acetylene glycol compound.

[0023] Further preferably, the organosilicon compound is selected from at least one of TEGO Wet 245, TEGO Wet 510 and TEGO Wet 500; the acetylene glycol compound is selected from at least one of Greesol A04BC and Greesol A04DPM produced by Yueyang Kaimen Company.

[0024] Preferably, the defoaming agent includes at least one of an organosilicon compound and a polyether compound.

[0025] Preferably, the defoaming agent is selected from at least one of TEGO Foamex825, TEGO Foamex810 and TEGO Foamex805.

[0026] Preferably, the solvent includes at least one of xylene and ethyl acetate.

[0027] The second aspect of the present invention provides a method for preparing the coating according to the first aspect of the present invention.

[0028] Specifically, the method for preparing the coating comprises the following steps:

[0029] The coating is prepared by mixing various raw material components.

[0030] Preferably, the methylphenyl modified silicone resin and the epoxy modified silicone resin are first mixed, and the accelerator, the wetting agent and the defoaming agent are added while stirring, and the stirring is continued, and then the solvent is added and the rotation speed is adjusted to obtain the coating.

[0031] Preferably, the stirring speed is 450-850 r / min; further preferably, the stirring speed is 500-800 r / min.

[0032] Preferably, the stirring time of the continued stirring is 9-22 min; further preferably, the stirring time of the continued stirring is 10-20 min.

[0033] Preferably, the rotation speed is adjusted to 270-550 r / min; further preferably, the rotation speed is adjusted to 300-500 r / min.

[0034] Preferably, the method for preparing the methylphenyl modified silicone resin comprises the following steps:

[0035] (1) mixing dimethyldichlorosilane, phenyltrichlorosilane, methyltrichlorosilane, a coupling agent, and a solvent to obtain a mixture;

[0036] (2) hydrolyzing the mixture obtained in step (1) to obtain a hydrolyzate, adding a catalyst to the hydrolyzate, heating in a water bath, adjusting the pH to neutral, and curing to obtain a vinyl-containing methylphenyl silicone resin;

[0037] (3) Mixing methacryloxypropyl cage silsesquioxane, an initiator and the vinyl-containing methylphenyl silicone resin obtained in step (2), reacting them, and distilling them under reduced pressure to obtain the methylphenyl-modified silicone resin.

[0038] Preferably, step (1) is specifically as follows: benzene, alcohol and water are mixed and heated in a water bath to obtain mixture 1; dimethyldichlorosilane, phenyltrichlorosilane, methyltrichlorosilane, a coupling agent and benzene are mixed to obtain mixture 2; and the mixture 1 and the mixture 2 are mixed to obtain the mixture.

[0039] Preferably, the benzene comprises toluene, and the alcohol comprises n-butanol.

[0040] Specifically, the mixture 1 functions to dissolve and disperse the mixture 2.

[0041] Preferably, stirring is performed under the water bath heating condition to obtain a mixture 1.

[0042] Preferably, the water bath heating temperature is 35-55°C, and the stirring time is 25-35min; further preferably, the water bath heating temperature is 40-50°C, and the stirring time is 27-33min; further preferably, the water bath heating temperature is 45°C, and the stirring time is 30min.

[0043] Preferably, in step (2), the hydrolysis temperature is 35-55°C, and the hydrolysis time is 0.8-1.2h; the water bath heating temperature is 45-65°C, and the water bath heating time is 15-25min; further preferably, in step (2), the hydrolysis temperature is 40-50°C, and the hydrolysis time is 0.9-1.1h; the water bath heating temperature is 50-60°C, and the water bath heating time is 18-22min; further preferably, in step (2), the hydrolysis temperature is 45°C, and the hydrolysis time is 1h; the water bath heating temperature is 55°C, and the water bath heating time is 20min.

[0044] Preferably, silanol is obtained after the hydrolysis, and then the silanol is washed with water until the pH of the filtrate is 6-7.

[0045] Preferably, in step (2), the catalyst comprises at least one of methacrylate, hydroxyethyl methacrylate and phosphoric acid.

[0046] Preferably, in step (2), a curing agent is added for curing, and the curing agent includes butyl titanate.

[0047] Preferably, in step (3), the reaction temperature is 45-65°C, and the reaction time is 15-25 min; further preferably, in step (3), the reaction temperature is 50-60°C, and the reaction time is 18-22 min; further preferably, in step (3), the reaction temperature is 55°C, and the reaction time is 20 min.

[0048] Specifically, in step (3), the reaction is carried out under heating in a water bath.

[0049] Specifically, the grafting reaction of methacryloxypropyl cage silsesquioxane (methacryl-poss) with silicone resin is carried out in the presence of an initiator, and the reaction temperature is high. Si-OH of silicone resin shrinks under high temperature conditions. Therefore, the resin modified with methacryl-poss can reduce or even avoid the "unbuttoning" degradation caused by Si-OH, and can reduce or even avoid the "unbuttoning" degradation caused by terminal hydroxyl groups, thereby improving the heat resistance of silicone resin.

[0050] Preferably, the mass ratio of the dimethyldichlorosilane, phenyltrichlorosilane, methyltrichlorosilane and coupling agent is (0.8-1.2): (1.7-2.5): (1-1.4): 1; further preferably, the mass ratio of the dimethyldichlorosilane, phenyltrichlorosilane, methyltrichlorosilane and coupling agent is (0.9-1.1): (1.9-2.3): (1.1-1.3): 1; further preferably, the mass ratio of the dimethyldichlorosilane, phenyltrichlorosilane, methyltrichlorosilane and coupling agent is 1:2.1:1.215:1.

[0051] Preferably, the mass ratio of the methacryloxypropyl cage silsesquioxane, the initiator and the coupling agent is (0.18-0.28): (0.65-0.90): 1; further preferably, the mass ratio of the methacryloxypropyl cage silsesquioxane, the initiator and the coupling agent is (0.2-0.25): (0.7-0.85): 1; further preferably, the mass ratio of the methacryloxypropyl cage silsesquioxane, the initiator and the coupling agent is 0.23: 0.77: 1.

[0052] Preferably, the coupling agent comprises a silane coupling agent.

[0053] Preferably, the initiator comprises dibenzoyl peroxide (BPO).

[0054] The third aspect of the present invention provides an application of the coating described in the first aspect of the present invention in the field of metal corrosion protection.

[0055] Compared with the prior art, the technical solution provided by the present invention has the following beneficial effects:

[0056] (1) The vinyl-containing methylphenyl silicone resin of the present invention can greatly reduce the number of terminal hydroxyl groups, and by using methacryloyloxypropyl cage-type silsesquioxane to modify the vinyl-containing methylphenyl silicone resin, the "unbuttoning" degradation caused by Si-OH of the silicone resin can be reduced or even avoided, and the "unbuttoning" degradation caused by the terminal hydroxyl groups can be reduced or even avoided, thereby improving the heat resistance of the silicone resin. The prepared coating produces a tight network structure after curing, and even under thermal stress, the cured coating can prevent cracks from forming. The present invention uses a compound of methylphenyl modified silicone resin and epoxy modified silicone resin, and the two work together to make the coating be prepared into a high film thickness coating. When the coating thickness is relatively thick, it still has good high temperature resistance, such as good adhesion, and is not easy to crack at high temperature, thereby facilitating construction operations. At the same time, because the coating of the present invention has good high temperature resistance, it does not need to add high temperature resistant fillers, such as aluminum powder, glass powder, mica powder, etc., and can be made into varnish.

[0057] (2) The grafting reaction of the methacryloxypropyl cage-type silsesquioxane (methacryl-poss) and the silicone resin of the present invention is carried out under the action of an initiator, and the reaction temperature is relatively high. The Si-OH of the silicone resin shrinks under high temperature conditions. Therefore, the resin modified with methacryl-poss can reduce or even avoid the "unbuttoning" type degradation caused by Si-OH, and can reduce or even avoid the "unbuttoning" type degradation caused by terminal hydroxyl groups, thereby improving the heat resistance of the silicone resin, and then improving the high temperature resistance of the coating, having good adhesion at high film thickness, and not easy to crack.

[0058] (3) The preparation process of the present invention is simple and convenient for large-scale production and application. DETAILED DESCRIPTION

[0059] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0060] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0061] Example 1

[0062] A coating, comprising 40 kg of methacryloyloxyphenyl silicone resin, 38 kg of epoxy modified silicone resin ES-1001N (Shin-Etsu, Japan), 3 kg of accelerator zinc isooctanoate, 0.5 kg of wetting agent TEGO Wet 500, 0.5 kg of defoaming agent TEGO Foamex 810 and 18 kg of solvent xylene;

[0063] Among them, the structural formula of methacryloyloxyphenyl silicone resin is:

[0064] Among them, R1 is methyl, R2 is phenyl, and n is 5500.

[0065] A method for preparing a coating comprises the following steps:

[0066] Add methacryloyloxyphenyl silicone resin and epoxy modified silicone resin into a dispersion tank, adjust the stirring speed to 500r / min, add accelerator, wetting agent and defoamer in sequence under stirring, then stir for 15 minutes, add xylene, adjust the stirring speed to 300r / min, stir evenly, and obtain silicone varnish with high film thickness and high temperature resistance, that is, the coating is prepared.

[0067] The preparation method of the methacryloyloxyphenyl silicone resin comprises the following steps:

[0068] (1) Add 13.00 g of toluene, 3.50 g of n-butanol, and 25.00 g of water into a round-bottom flask, and stir thoroughly for 30 min in a water bath at 45° C. to obtain a mixed solvent;

[0069] (2) dissolving 1.31 g of dimethyldichlorosilane, 2.73 g of phenyltrichlorosilane, 1.58 g of methyltrichlorosilane and 1.3 g of silane coupling agent (KH570) monomer in 7.00 g of toluene solvent in turn to obtain a mixed solution; adding the mixed solvent dropwise to the round-bottom flask containing the mixed solvent in step (1), heating in a water bath at 45° C. for hydrolysis and stirring for 1 h; washing the silanol obtained by hydrolysis with water until the pH of the filtrate is 6-7, pouring the washed silanol into a flask, adding 0.40 g of 10% methyl acrylate, heating and stirring in a water bath at 55° C. for 20 min; finally, adding a small amount of acetic acid, stirring well, adjusting the solution pH to 7, adding a small amount of curing agent butyl titanate, stirring and ultrasonicating for 30 min each, pouring into a mold, and curing at room temperature to obtain a vinyl-containing methylphenyl silicone resin;

[0070] (3) adding methacryloxypropyl cage-type silsesquioxane and BPO initiator to the vinyl-containing methylphenyl silicone resin obtained in step (2), stirring to uniformly mix the three, stirring for 20 minutes under heating conditions at 55° C. in a water bath to allow the vinyl-containing methylphenyl silicone resin and methacryloxypropyl cage-type silsesquioxane to fully react, and then performing reduced pressure distillation to obtain a methacryloxyphenyl silicone resin.

[0071] Example 2

[0072] A coating comprises 41 kg of methacryloyloxyphenyl silicone resin, 37 kg of epoxy modified silicone resin ES-1001N, 3 kg of accelerator zinc isooctanoate, 0.5 kg of wetting agent TEGO Wet 500, 0.5 kg of defoaming agent TEGO Foamex805 and 18 kg of xylene.

[0073] The method for preparing the coating comprises the following steps:

[0074] Add methacryloyloxyphenyl silicone resin and epoxy modified silicone resin into a dispersion tank, adjust the stirring speed to 500 r / min, add accelerator zinc isooctanoate, wetting agent TEGO Wet 500, and defoaming agent TEGOFoamex805 in sequence under stirring, then stir for 15 minutes, add xylene, adjust the stirring speed to 300 r / min, stir evenly, and obtain a silicone varnish with high film thickness and high temperature resistance, that is, a coating.

[0075] The structural formula and preparation method of the methacryloyloxyphenyl silicone resin in Example 2 are the same as those in Example 1.

[0076] Example 3

[0077] A coating comprises 41 kg of methacryloyloxyphenyl silicone resin, 37 kg of epoxy-modified silicone resin ES-1001N, 3 kg of accelerator zinc isooctanoate, 0.5 kg of wetting agent TEGO Wet 245, 0.5 kg of defoaming agent TEGO Foamex80 and 18 kg of xylene.

[0078] The method for preparing the coating comprises the following steps:

[0079] Add methacryloyloxyphenyl silicone resin and epoxy modified silicone resin into a dispersion tank, adjust the stirring speed to 500 r / min, add accelerator zinc isooctanoate, wetting agent TEGO Wet 245, and defoaming agent TEGOFoamex805 in sequence under stirring, then stir for 15 minutes, add xylene, adjust the stirring speed to 300 r / min, stir evenly, and obtain a silicone varnish with high film thickness and high temperature resistance, that is, a coating.

[0080] The structural formula and preparation method of the methacryloxyphenyl silicone resin in Example 3 are the same as those in Example 1.

[0081] Comparative Example 1

[0082] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 uses methyl silicone resin to replace the methacryloyloxyphenyl silicone resin and the epoxy-modified silicone resin in equal amounts, and the rest is the same as Example 1.

[0083] Comparative Example 2

[0084] The difference between Comparative Example 2 and Example 1 is that Comparative Example 2 uses methylphenyl silicone resin to replace the methacryloyloxyphenyl silicone resin and the epoxy-modified silicone resin in equal amounts, and the rest is the same as Example 1.

[0085] Comparative Example 3

[0086] The difference between Comparative Example 3 and Example 1 is that Comparative Example 3 uses an equal amount of epoxy-modified silicone resin to replace the methacryloxyphenyl silicone resin, and the rest is the same as Example 1.

[0087] Comparative Example 4

[0088] The difference between Comparative Example 4 and Example 1 is that Comparative Example 4 uses an equal amount of methacryloxyphenyl silicone resin to replace the epoxy modified silicone resin, and the rest is the same as Example 1.

[0089] Performance Testing

[0090] The coatings prepared in Examples 1-3 and Comparative Examples 1-4 were sprayed on sandblasted steel plates respectively by spray guns, and each group obtained a paint film with a thickness of 10-20 μm, 20-30 μm, 30-40 μm, 50-60 μm, and 60-70 μm. After the sandblasted steel plates were dried for 7 days, they were placed in an oven, baked at 250°C for 3 hours, taken out, cooled at room temperature, and then subjected to performance tests. The test items and test methods are as follows:

[0091] Paint film appearance: visual;

[0092] Adhesion: refer to GB / T 9286-2021;

[0093] Impact test: refer to GB / T1732-1993.

[0094] The performance test results of the coatings prepared in Examples 1-3 are shown in Table 1, and the performance test results of the coatings prepared in Comparative Examples 1-4 are shown in Table 2.

[0095] Table 1: Performance test results of the coatings prepared in Examples 1-3

[0096]

[0097] Table 2: Performance test results of the coatings prepared in Comparative Examples 1-4

[0098]

[0099] As can be seen from Table 1, the paint film with a thickness of 10-60 μm obtained by spraying the paint of the present invention has a normal appearance, no cracks, good adhesion, and no cracking after the impact test, indicating that the paint of the present invention has good high temperature resistance.

[0100] As shown in Tables 1 and 2, Comparative Example 1 uses methyl silicone resin to replace methacryloyloxyphenyl silicone resin and epoxy modified silicone resin in equal amounts, so that when the film thickness of Comparative Example 1 is thin (10-20 μm), the impact test shows good adhesion and no obvious cracking of the paint film, but when the film thickness is thick (20-60 μm), cracking occurs in the impact test, the adhesion can reach level 4, the adhesion is poor, and the paint film cracks seriously. This shows that the high temperature resistance of the coating of Comparative Example 1 is significantly worse than that of Example 1, especially the high temperature resistance at high film thickness is significantly worse than that of Example 1.

[0101] Comparative Example 2 uses methylphenyl silicone resin to replace methacryloyloxyphenyl silicone resin and epoxy modified silicone resin in equal amounts, so that when the paint film thickness of Comparative Example 2 is 20-30μm, the adhesion is worse than that of Example 1, and when the paint film is thicker (30-60μm), cracking occurs in the impact test, and the adhesion can reach level 4, the adhesion is poor, and the paint film cracks severely, indicating that the high temperature resistance of the coating of Comparative Example 2 is significantly worse than that of Example 1, especially the high temperature resistance at high film thickness is significantly worse than that of Example 1.

[0102] Comparative Example 3 uses an equal amount of epoxy-modified silicone resin to replace the methacryloyloxyphenyl silicone resin, so that when the film thickness of Comparative Example 3 is thin (10-20 μm), the impact test shows good adhesion and no obvious cracking of the paint film, but when the film thickness is thick (20-60 μm), cracking occurs in the impact test, the adhesion can reach level 4, the adhesion is poor, and the paint film cracks. It shows that the high temperature resistance of the coating of Comparative Example 3 is significantly worse than that of Example 1, especially when the paint film is thick.

[0103] Comparative Example 4 uses an equal amount of methacryloyloxyphenyl silicone resin to replace the epoxy modified silicone resin, so that when the film thickness of Comparative Example 4 is 10-30 μm, the impact test and the appearance of the paint film are normal, but the adhesion of the paint film is worse than that of Example 1, and as the thickness of the paint film increases, when the thickness of the paint film is 30-60 μm, cracking occurs after the impact test, the adhesion is poor (can reach level 4), and the appearance of the paint film is cracked. It shows that the high temperature resistance of the coating of Comparative Example 4 is significantly worse than that of Example 1, especially when the paint film is thicker.

[0104] In summary, the present invention uses methacryloxypropyl cage silsesquioxane to modify the vinyl-containing methylphenyl silicone resin, and through the compounding of methylphenyl modified silicone resin and epoxy modified silicone resin, the two work together to make the coating be prepared into a high film thickness coating, and when the coating thickness is thick, it still has good high temperature resistance, such as good adhesion, not easy to crack at high temperature, and the coating does not crack after impact test, thereby facilitating construction operation. At the same time, because the coating of the present invention has good high temperature resistance, it does not need to add high temperature resistant fillers, such as aluminum powder, glass powder, mica powder, etc., and can be made into varnish.

[0105] The above embodiments are only used to illustrate the technical solution of the present invention rather than to limit the protection scope of the present invention. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solution of the present invention can be modified or replaced by equivalents without departing from the essence and scope of the technical solution of the present invention.

Claims

1. A coating, characterized in that: Including methylphenyl modified silicone resin, epoxy modified silicone resin; The methylphenyl modified silicone resin is obtained by modifying a vinyl-containing methylphenyl silicone resin with methacryloxypropyl cage-type silsesquioxane.

2. The coating according to claim 1, characterized in that The structural formula of the methylphenyl modified silicone resin is: Wherein, the R1 is selected from any one of methyl and phenyl, the R2 is selected from any one of methyl and phenyl, and the R1 and R2 are different; and the n is 4000-6000.

3. The coating according to claim 1, characterized in that The coating further comprises at least one of an auxiliary agent and a solvent.

4. The coating according to claim 3, characterized in that The auxiliary agent includes at least one of a promoter, a wetting agent and a defoaming agent.

5. The coating according to claim 4, characterized in that The coating also includes an accelerator, a wetting agent, a defoamer and a solvent; and by mass percentage, the coating includes 36-45% of methylphenyl modified silicone resin, 36-45% of epoxy modified silicone resin, 0.5-3.3% of accelerator, 0.2-0.55% of wetting agent, 0.2-0.55% of defoamer and 5.6-27.1% of solvent.

6. The method for preparing the coating according to any one of claims 1 to 5, characterized in that: The following steps are involved: The coating is prepared by mixing various raw material components.

7. The preparation method according to claim 6, characterized in that: The preparation method of the methylphenyl modified silicone resin comprises the following steps: (1) mixing dimethyldichlorosilane, phenyltrichlorosilane, methyltrichlorosilane, a coupling agent, and a solvent to obtain a mixture; (2) hydrolyzing the mixture obtained in step (1) to obtain a hydrolyzate, adding a catalyst to the hydrolyzate, heating in a water bath, adjusting the pH to neutral, and curing to obtain a vinyl-containing methylphenyl silicone resin; (3) Mixing methacryloxypropyl cage silsesquioxane, an initiator and the vinyl-containing methylphenyl silicone resin obtained in step (2), reacting them, and distilling them under reduced pressure to obtain the methylphenyl-modified silicone resin.

8. The preparation method according to claim 7, characterized in that: Step (1) specifically comprises mixing benzene, alcohol and water, and heating in a water bath to obtain a mixture 1; mixing dimethyldichlorosilane, phenyltrichlorosilane, methyltrichlorosilane, a coupling agent and benzene to obtain a mixture 2; and mixing the mixture 1 and the mixture 2 to obtain the mixture; And / or, in step (2), the hydrolysis temperature is 35-55°C, and the hydrolysis time is 0.8-1.2h; the water bath heating temperature is 45-65°C, and the water bath heating time is 15-25min; And / or, in step (3), the reaction temperature is 45-65°C, and the reaction time is 15-25 min.

9. The preparation method according to claim 7, characterized in that: The mass ratio of dimethyldichlorosilane, phenyltrichlorosilane, methyltrichlorosilane and coupling agent is (0.8-1.2): (1.7-2.5): (1-1.4): 1; And / or, the mass ratio of the methacryloxypropyl cage silsesquioxane, the initiator and the coupling agent is (0.18-0.28):(0.65-0.90):

1.

10. Use of the coating according to any one of claims 1 to 6 in the field of metal corrosion protection.

Citation Information

Patent Citations

  • A silicone resin composition and uses thereof

    CN106554621A

  • Preparation method for methylphenyl silicone resin and coating

    CN108707231A