Environment-friendly water-based halogen-free flame-retardant pressure-sensitive adhesive and preparation method thereof

The preparation of flame retardant monomers and tackifier monomers containing ternary flame retardant elements of silicon, nitrogen and phosphorus through emulsion polymerization has solved the problem of poor flame retardant performance of acrylic resin pressure-sensitive adhesives, and achieved excellent flame retardant and bonding Performance expands its application scope.

CN119081604APending Publication Date: 2024-12-06CROWN NEW MATERIALS TECHNOLOGY CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411433464.1
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-10-15
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The flame retardant properties of acrylic resin pressure-sensitive adhesives are poor, which limits their applications in electronics, automobiles and construction fields.

Method used

Flame retardant monomers and tackifying monomers are prepared by emulsion polymerization. By tetramethyldisilazane, pentaerythritol phosphate, allyl epoxy end-capped polyether and other materials, it forms a ternary resistor containing silicon, nitrogen and phosphorus. Flame-retardant monomer of combustion elements, and viscosity-enhancing monomers are prepared by materials such as 1,5-hexadiene-3,4-diol, 2,2'-dibromodyethyl ether, and polymerized with emulsifier and initiator. , an environmentally friendly water-friendly halogen-free flame-retardant pressure-sensitive adhesive with excellent flame retardant and bonding properties is formed.

Benefits of technology

The flame retardant and bonding properties of acrylic resin pressure-sensitive adhesives are improved, and their application range is expanded. They can quickly generate an expanded carbon layer to prevent combustion when fire occurs, and enhance bonding properties through polyether segments.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119081604A_ABST
    Figure CN119081604A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of adhesives, and discloses an environment-friendly water-based halogen-free flame-retardant pressure-sensitive adhesive and a preparation method thereof.The pressure-sensitive adhesive is prepared from a soft monomer, a hard monomer, a flame-retardant monomer, a tackifying monomer and other raw materials through emulsion polymerization under the action of an initiator, the flame-retardant monomer can participate in the free radical copolymerization reaction of acrylic resin, and the tackifying monomer can participate in the free radical copolymerization reaction of acrylic resin; the polyether chain segment can exist in an acrylic resin pressure-sensitive adhesive molecular chain in a chemical connection mode, the pressure-sensitive adhesive is endowed with excellent flame retardant performance, the polyether chain segment can improve the bonding performance of the pressure-sensitive adhesive, the molecular chain of acrylic resin can be converted into a three-dimensional network structure from a straight-chain structure through the addition of the tackifying monomer, and the flame retardant property of the pressure-sensitive adhesive is improved. According to the present invention, the cross-linking density of the acrylic resin molecular chain is improved, the cohesive force of the pressure-sensitive adhesive is effectively improved so as to enhance the adhesive property of the pressure-sensitive adhesive, and the number of the hydrogen bonds between the pressure-sensitive adhesive and the adhered object can be increased by the large amount of the ether bonds contained in the tackifying monomer so as to further improve the adhesive property of the pressure-sensitive adhesive.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of adhesives, and in particular to an environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive and a preparation method thereof. Background Art

[0002] In today's society, environmental protection has become an important issue that cannot be ignored in all walks of life. In the field of adhesives, since traditional solvent-based adhesives will volatilize organic solvents, which is not conducive to environmental protection, their application is gradually limited. Environmentally friendly water-based pressure-sensitive adhesives are gradually replacing traditional solvent-based adhesives due to their unique environmental characteristics and broad application prospects. Among them, acrylic resin pressure-sensitive adhesives, as an important representative of environmentally friendly water-based pressure-sensitive adhesives, not only meet environmental protection requirements, but also have a series of excellent properties.

[0003] As acrylic resin pressure-sensitive adhesives are widely used in electronics, automobiles, construction and other fields, the shortcomings of acrylic resin pressure-sensitive adhesives, such as poor flame retardancy, are fully exposed due to the high requirements for safety performance in these fields. This has a significant negative impact on the continued application of acrylic resin pressure-sensitive adhesives. Therefore, there is an urgent need to improve the functionality of acrylic resin pressure-sensitive adhesives, such as flame retardancy.

[0004] The invention patent with application number CN202111591645.3 discloses a method for preparing a low-VOC halogen-free flame-retardant pressure-sensitive adhesive. Ultrafine ammonium polyphosphate particles are prepared and used as a flame retardant to enhance the flame retardant properties of acrylic resin pressure-sensitive adhesive. Therefore, the formula of the acrylic resin pressure-sensitive adhesive can be designed to give the acrylic resin pressure-sensitive adhesive more functionality. Based on this, the present invention provides an acrylic resin pressure-sensitive adhesive. By designing the acrylic resin molecular chain, the prepared pressure-sensitive adhesive has good halogen-free flame retardancy and other functionalities, which can further expand the application scope of the acrylic resin pressure-sensitive adhesive. Summary of the invention

[0005] In order to solve the problems mentioned in the background technology, the purpose of the present invention is to provide an environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive and a preparation method thereof.

[0006] The purpose of the present invention can be achieved through the following technical solutions:

[0007] A method for preparing an environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive, wherein the pressure-sensitive adhesive is made of the following raw materials in parts by weight:

[0008]

[0009] The preparation method comprises the following steps:

[0010] Step 1: weigh each raw material according to weight and set aside;

[0011] Step 2: adding an emulsifier and two-thirds of purified water into a polymerization kettle, stirring and mixing, and then adding a soft monomer, a hard monomer, a flame retardant monomer and a viscosity-increasing monomer into the polymerization kettle, stirring and mixing thoroughly to form an emulsion;

[0012] Step 3, adding the initiator to the remaining amount of purified water, stirring and mixing to form a mixed solution;

[0013] Step 4: Add the mixed solution to the emulsion, introduce nitrogen for protection, then gradually increase the temperature to 78-82°C, keep warm for 6-9 hours, remove the nitrogen, stop heating, and discharge the material.

[0014] As a further embodiment of the present invention, the soft monomer is at least one of ethyl acrylate, n-butyl acrylate or lauryl methacrylate; the hard monomer is at least one of isobornyl methacrylate, styrene, acrylonitrile and methyl methacrylate.

[0015] In the above technical solution, the acrylic resin pressure-sensitive adhesive is obtained by adopting emulsion polymerization method, using soft monomers, hard monomers, flame-retardant monomers and tackifying monomers as free radical copolymers and carrying out emulsion polymerization under the action of an initiator.

[0016] As a further solution of the present invention, the flame retardant monomer is prepared by the following method:

[0017] Step ①, adding tetramethyldisilazane, pentaerythritol phosphate and toluene into a reaction kettle, starting stirring, mixing evenly, introducing nitrogen protection, and dripping trifluoroacetic acid catalyst, after the addition, gradually raising the temperature to 95-100° C., and heat-insulating for 4-8 hours to obtain a flame retardant intermediate material;

[0018] Step ②, mix the allyl epoxy terminated polyether and tetrahydrofuran, stir until a uniform liquid is formed, then add the flame retardant intermediate material to the liquid, turn on the heating after the addition, wait for the temperature to rise to 60-65°C, and keep it at this temperature for 2-4 hours to obtain the flame retardant monomer.

[0019] As a further embodiment of the present invention, in step ①, the molar ratio of tetramethyldisilazane to pentaerythritol phosphate is 1:2.

[0020] As a further embodiment of the present invention, in step ②, the number average molecular weight of the allyl epoxy terminated polyether is 1000.

[0021] In the above technical scheme, under the action of a catalyst, Si-H in the tetramethyldisilazane structure can react with the substituted hydroxyl group of pentaerythritol phosphate to obtain a flame retardant intermediate containing ternary flame retardant elements of silicon, nitrogen and phosphorus in its structure, and the secondary amine group in its structure can further undergo ring-opening addition with the epoxy group in the allyl epoxy-terminated polyether structure to obtain a flame retardant monomer.

[0022] As a further embodiment of the present invention, the preparation method of the viscosity-increasing monomer is as follows:

[0023] Add 1,5-hexadiene-3,4-diol to 1,4-dioxane solvent and start stirring until a uniform solution is formed, then add sodium hydroxide solution. After the addition is completed, introduce nitrogen to evacuate the air, and then add 2,2'-dibromodiethyl ether to the solution. After the addition is completed, start heating and control the temperature at 70-80°C. Keep the temperature for 8-12 hours under continuous stirring, remove nitrogen, evaporate and remove the solvent, cool and discharge the material to obtain a viscosity-enhancing monomer.

[0024] As a further embodiment of the present invention, the molar ratio of 1,5-hexadiene-3,4-diol to 2,2'-dibromodiethyl ether is 1:0.8-1.

[0025] As a further solution of the present invention, the mass fraction of the sodium hydroxide solution is 25-35%.

[0026] In the above technical scheme, the hydroxyl groups in the 1,5-hexadiene-3,4-diol structure are activated by using sodium hydroxide, and then an uninterrupted substitution reaction is carried out with 2,2'-dibromodiethyl ether under high temperature conditions to form a polymeric molecule connected by ether bonds and having an alternating connection structure, namely a viscosity-enhancing monomer.

[0027] As a further embodiment of the present invention, the emulsifier is sodium dodecylbenzene sulfonate or sodium dodecyl sulfate; the initiator is at least one of potassium persulfate, sodium persulfate or ammonium persulfate.

[0028] An environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive is prepared by adopting the preparation method.

[0029] Beneficial effects of the present invention:

[0030] (1) One end of the flame retardant monomer structure prepared by the present invention contains an alkenyl substituent that can participate in the free radical copolymerization reaction of acrylic resin, so it can exist in the molecular chain of acrylic resin pressure-sensitive adhesive in a chemically connected manner. Since the flame retardant monomer structure contains ternary flame retardant elements of silicon, nitrogen and phosphorus at the same time, it can quickly produce an expanded carbon layer containing silicon oxide when a fire occurs, forming protection for the interior in time, preventing the combustion from continuing, and making it difficult for the fire to spread, thereby giving the pressure-sensitive adhesive excellent flame retardant properties. In addition, the polyether segment contained in the flame retardant monomer structure can also play a positive effect on enhancing the bonding performance of the pressure-sensitive adhesive.

[0031] (2) The tackifying monomer prepared by the present invention contains a plurality of unsaturated olefinic substituents in its structure, and thus can act as a cross-linking agent in the process of free radical copolymerization, and can transform the molecular chain of the acrylic resin from a linear structure to a three-dimensional network structure, thereby increasing the cross-linking density of the acrylic resin molecular chain, and effectively improving the cohesive force of the pressure-sensitive adhesive, thereby enhancing the bonding performance of the pressure-sensitive adhesive. In addition, the large number of ether bonds contained in the tackifying monomer can increase the number of hydrogen bonds between the pressure-sensitive adhesive and the adhered object, thereby further improving the bonding performance of the pressure-sensitive adhesive.

[0032] Of course, any product implementing the present invention does not necessarily need to achieve all of the advantages described above at the same time. BRIEF DESCRIPTION OF THE DRAWINGS

[0033] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the accompanying drawings required for describing the embodiments will be briefly introduced below. Obviously, the accompanying drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other accompanying drawings can be obtained based on these accompanying drawings without paying creative work.

[0034] Figure 1 This is the infrared analysis test chart of the flame retardant monomer;

[0035] Figure 2 This is the infrared analysis test chart of the viscosity-increasing monomer. DETAILED DESCRIPTION

[0036] The following will be combined with the drawings in the embodiments of the present invention to clearly and completely describe the technical solutions in the embodiments of the present invention. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0037] Preparation Example 1

[0038] Preparation of flame retardant monomers:

[0039] Step ①, add 0.4g tetramethyldisilazane, 1.08g pentaerythritol phosphate and toluene into the reaction kettle, start stirring, mix evenly, introduce nitrogen protection, and drop 0.1g trifluoroacetic acid, after the addition, gradually increase the temperature to 100°C, keep warm for 6h, and obtain a flame retardant intermediate material;

[0040] Step ②, mix 1.2g of allyl epoxy-terminated polyether with a number average molecular weight of 1000 and tetrahydrofuran, stir to form a uniform liquid, then add 0.6g of flame retardant intermediate material to the liquid, turn on the heating after adding, wait for the temperature to rise to 60°C, and keep it at this temperature for 3h to obtain the flame retardant monomer.

[0041] Figure 1 This is the infrared analysis test chart of the flame retardant monomer, where 3293cm -1 The characteristic absorption peak of hydroxyl group is 3032cm -1 The CH characteristic absorption peak of unsaturated carbon-carbon double bond is 2800~3000cm -1 The CH characteristic absorption peaks of methyl and methylene are at 1279 cm -1 The P=O characteristic absorption peak is at 1000~1100cm -1 The characteristic absorption peaks of Si-O and COC overlap with each other.

[0042] Preparation Example 2

[0043] The viscosity-increasing monomer was prepared by the following method:

[0044] 0.6 g of 1,5-hexadiene-3,4-diol was added to 1,4-dioxane solvent and stirred until a uniform solution was formed. Then, 5 mL of 30% sodium hydroxide solution was added. After the addition was completed, nitrogen was introduced to exhaust the air. Then, 0.8 g of 2,2'-dibromodiethyl ether was added to the solution. After the addition was completed, heating was started and the temperature was controlled at 75°C. The solution was kept warm for 9 hours under continuous stirring. The nitrogen was removed, the solvent was evaporated and removed, and the temperature was lowered to obtain a viscosity-enhancing monomer.

[0045] Figure 2 This is the infrared analysis test chart of the viscosity-enhancing monomer, where 3405cm -1 The characteristic absorption peak of hydroxyl group provided by excess 1,5-hexadiene-3,4-diol is 3060cm -1 The characteristic absorption peak of CH on the unsaturated carbon-carbon double bond is 1080cm -1 The absorption peak at the center is the characteristic absorption peak of ether bond COC.

[0046] Example 1

[0047] An environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive is made of the following raw materials in parts by weight:

[0048]

[0049]

[0050] The preparation method of the pressure-sensitive adhesive comprises the following steps:

[0051] Step 1: weigh each raw material according to weight and set aside;

[0052] Step 2: adding sodium dodecylbenzene sulfonate and two-thirds of purified water into a polymerization kettle, stirring and mixing, and then adding ethyl acrylate, isobornyl methacrylate, a flame retardant monomer and a viscosity-increasing monomer into the polymerization kettle, stirring and mixing thoroughly to form an emulsion;

[0053] Step 3, adding potassium persulfate to the remaining amount of purified water, stirring and mixing to form a mixed solution;

[0054] Step 4: Add the mixed solution to the emulsion, introduce nitrogen for protection, then gradually increase the temperature to 78°C, keep warm for 9 hours, remove the nitrogen, stop heating, and discharge the material.

[0055] The preparation method of the flame retardant monomer is shown in Preparation Example 1, and the preparation method of the viscosity-increasing monomer is shown in Preparation Example 2, and the same shall apply to the following.

[0056] Example 2

[0057] An environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive is made of the following raw materials in parts by weight:

[0058]

[0059]

[0060] The preparation method of the pressure-sensitive adhesive comprises the following steps:

[0061] Step 1: weigh each raw material according to weight and set aside;

[0062] Step 2: adding sodium dodecyl sulfate and two-thirds of purified water into a polymerization kettle, stirring and mixing, and then adding n-butyl acrylate, methyl methacrylate, flame retardant monomer and viscosity-increasing monomer into the polymerization kettle, stirring and mixing thoroughly to form an emulsion;

[0063] Step 3, adding sodium persulfate to the remaining amount of purified water, stirring and mixing to form a mixed solution;

[0064] Step 4: Add the mixed solution to the emulsion, introduce nitrogen for protection, then gradually increase the temperature to 80°C, keep warm for 8 hours, remove the nitrogen, stop heating, and discharge the material.

[0065] Example 3

[0066] An environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive is made of the following raw materials in parts by weight:

[0067]

[0068] The preparation method of the pressure-sensitive adhesive comprises the following steps:

[0069] Step 1: weigh each raw material according to weight and set aside;

[0070] Step 2: adding sodium dodecylbenzene sulfonate and two-thirds of purified water into a polymerization kettle, stirring and mixing, and then adding lauryl methacrylate, styrene, flame retardant monomer and viscosity-increasing monomer into the polymerization kettle, stirring and mixing thoroughly to form an emulsion;

[0071] Step 3, adding ammonium persulfate to the remaining amount of purified water, stirring and mixing to form a mixed solution;

[0072] Step 4: Add the mixed solution to the emulsion, introduce nitrogen for protection, then gradually increase the temperature to 82°C, keep warm for 6 hours, remove the nitrogen, stop heating, and discharge the material.

[0073] Comparative Example 1

[0074] An environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive is made of the following raw materials in parts by weight:

[0075]

[0076] The preparation method of the pressure-sensitive adhesive comprises the following steps:

[0077] Step 1: weigh each raw material according to weight and set aside;

[0078] Step 2: adding sodium dodecyl sulfate and two-thirds of purified water into a polymerization kettle, stirring and mixing, and then adding n-butyl acrylate, methyl methacrylate and a viscosity-increasing monomer into the polymerization kettle, stirring and mixing thoroughly to form an emulsion;

[0079] Step 3, adding sodium persulfate to the remaining amount of purified water, stirring and mixing to form a mixed solution;

[0080] Step 4: Add the mixed solution to the emulsion, introduce nitrogen for protection, then gradually increase the temperature to 80°C, keep warm for 8 hours, remove the nitrogen, stop heating, and discharge the material.

[0081] Comparative Example 2

[0082] An environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive is made of the following raw materials in parts by weight:

[0083]

[0084] The preparation method of the pressure-sensitive adhesive comprises the following steps:

[0085] Step 1: weigh each raw material according to weight and set aside;

[0086] Step 2: adding sodium dodecyl sulfate and two-thirds of purified water into a polymerization kettle, stirring and mixing, and then adding n-butyl acrylate, methyl methacrylate, and a flame retardant monomer into the polymerization kettle, stirring and mixing thoroughly to form an emulsion;

[0087] Step 3, adding sodium persulfate to the remaining amount of purified water, stirring and mixing to form a mixed solution;

[0088] Step 4: Add the mixed solution to the emulsion, introduce nitrogen for protection, then gradually increase the temperature to 80°C, keep warm for 8 hours, remove the nitrogen, stop heating, and discharge the material.

[0089] Test Case

[0090] a. Pour the pressure-sensitive adhesives in Examples 1 to 3 and Comparative Examples 1 to 2 into a mold, cure at 100° C. for 10 min, and then age at 60° C. for 24 h, remove from the mold, and make test pieces that meet the specifications. Test the flame retardancy according to standard GB / T 2408-2021;

[0091] b. The pressure-sensitive adhesives in Examples 1 to 3 and Comparative Examples 1 to 2 were uniformly coated on PET release paper to a thickness of 50 μm, and then placed at 100° C. for curing for 10 min, and then aged at 60° C. for 24 h to prepare pressure-sensitive adhesive tapes. The 180° peel strength was tested according to the standard GB / T2792-2014;

[0092] The results are recorded in Table 1:

[0093] Table 1 - Test results

[0094] Flame retardant grade Peel strength / N / 25mm Example 1 V-0 6.1 Comparative Example 2 V-0 6.4 Example 3 V-0 6.2 Comparative Example 1 V-2 5.6 Comparative Example 2 V-0 3.9

[0095] The analysis and test results show that the pressure-sensitive adhesive prepared by adding flame retardant monomers and tackifying monomers exhibits excellent flame retardant and adhesive properties. After removing the flame retardant monomer, not only the flame retardant properties of the pressure-sensitive adhesive are greatly reduced, but also the loss of the polyether segment causes a slight decrease in the adhesive properties of the pressure-sensitive adhesive. After removing the tackifying monomer, the adhesive properties are greatly reduced.

[0096] Specific examples are used herein to illustrate the principles and implementation methods of the present invention. The description of the above embodiments is only used to help understand the method of the present invention and its core ideas, including the best mode, and also enable any technician in the field to practice the present invention, including making and using any device or system, and implementing any combined method. It should be pointed out that for ordinary technicians in this technical field, without departing from the principle of the present invention, the present invention can also be improved and modified, and these improvements and modifications also fall within the scope of protection of the claims of the present invention. The scope of patent protection of the present invention is defined by the claims and may include other embodiments that can be thought of by those skilled in the art. If these other embodiments have structural elements similar to the literal expression of the claims, or if they include equivalent structural elements that are not substantially different from the literal expression of the claims, then these other embodiments should also be included in the scope of the claims.

Claims

1. A method for preparing an environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive. It is characterized in that The pressure-sensitive adhesive is made of the following raw materials in parts by weight: The preparation method comprises the following steps: Step 1: weigh each raw material according to weight and set aside; Step 2: adding an emulsifier and two-thirds of purified water into a polymerization kettle, stirring and mixing, and then adding a soft monomer, a hard monomer, a flame retardant monomer and a viscosity-increasing monomer into the polymerization kettle, stirring and mixing thoroughly to form an emulsion; Step 3, adding the initiator to the remaining amount of purified water, stirring and mixing to form a mixed solution; Step 4: Add the mixed solution to the emulsion, introduce nitrogen for protection, then gradually increase the temperature to 78-82°C, keep warm for 6-9 hours, remove the nitrogen, stop heating, and discharge the material.

2. A method for preparing an environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive according to claim 1, It is characterized in that The soft monomer is at least one of ethyl acrylate, n-butyl acrylate or lauryl methacrylate; the hard monomer is at least one of isobornyl methacrylate, styrene, acrylonitrile and methyl methacrylate.

3. The method for preparing an environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive according to claim 1, It is characterized in that The flame retardant monomer is prepared by the following method: Step ①, adding tetramethyldisilazane, pentaerythritol phosphate and toluene into a reaction kettle, starting stirring, mixing evenly, introducing nitrogen protection, and dripping trifluoroacetic acid, after the addition, gradually raising the temperature to 95-100° C., and heat-insulating for 4-8 hours to obtain a flame retardant intermediate material; Step ②, mix the allyl epoxy terminated polyether and tetrahydrofuran, stir until a uniform liquid is formed, then add the flame retardant intermediate material to the liquid, turn on the heating after the addition, wait for the temperature to rise to 60-65°C, and keep it at this temperature for 2-4 hours to obtain the flame retardant monomer.

4. A method for preparing an environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive according to claim 3, It is characterized in that In step ①, the molar ratio of tetramethyldisilazane to pentaerythritol phosphate is 1:

2.

5. The method for preparing an environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive according to claim 3, It is characterized in that In step ②, the number average molecular weight of the allyl epoxy terminated polyether is 1000.

6. The method for preparing an environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive according to claim 1, It is characterized in that The preparation method of the viscosity-increasing monomer is as follows: Add 1,5-hexadiene-3,4-diol to 1,4-dioxane solvent and start stirring until a uniform solution is formed, then add sodium hydroxide solution. After the addition is completed, introduce nitrogen to evacuate the air, and then add 2,2'-dibromodiethyl ether to the solution. After the addition is completed, start heating and control the temperature at 70-80°C. Keep the temperature for 8-12 hours under continuous stirring, remove nitrogen, evaporate and remove the solvent, cool and discharge the material to obtain a viscosity-enhancing monomer.

7. A method for preparing an environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive according to claim 6, It is characterized in that The molar ratio of the 1,5-hexadiene-3,4-diol to 2,2'-dibromodiethyl ether is 1:0.8-1.

8. The method for preparing an environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive according to claim 6, It is characterized in that The mass fraction of the sodium hydroxide solution is 25-35%.

9. The method for preparing an environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive according to claim 1, It is characterized in that The emulsifier is sodium dodecylbenzene sulfonate or sodium dodecyl sulfate; the initiator is at least one of potassium persulfate, sodium persulfate or ammonium persulfate.

10. An environmentally friendly water-based halogen-free flame-retardant pressure-sensitive adhesive, It is characterized in that The compound is prepared by the preparation method as described in any one of claims 1 to 9.