Detachable polyurethane hot melt adhesive and preparation method thereof
By adding specific ingredients to the polyurethane hot melt adhesive and irradiating with UV light, the easy disassembly of the adhesive after UV light is achieved, the problem of difficult disassembly at high temperatures in the prior art is solved, and the disassembly of the adhesive is improved performance and performance.
Patent Information
- Application Number
- CN202411411620.4
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-10-11
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-10-11
AI Technical Summary
The existing reactive polyurethane hot melt adhesive is difficult to disassemble at high temperatures and cannot meet the easy disassembly of adhesives in electronic products and other industries.
Under UV light conditions, the adhesive is realized by adding polyol polymers, isocyanate compounds, modified resins, thermoplastic resins, tackifying resins, thermal fillers and latent curing agents to the polyurethane hot melt adhesive, and combining with photoinitiators to realize the adhesive Easy to disassemble.
After UV light exposure, the alicyclic epoxy resin undergoes polymerization reaction, which increases the colloid strength and reduces the peel strength, making the adhesive easier to disassemble. At the same time, the thermally conductive material transfers heat evenly, reduces the colloid temperature and enhances decomposition.
Smart Images

Figure SMS_1
Abstract
Description
Technical Field
[0001] The invention relates to a reactive polyurethane hot melt adhesive, in particular to a disassembled polyurethane hot melt adhesive and a preparation method thereof. Background Art
[0002] Reactive polyurethane hot melt adhesive is an environmentally friendly hot melt adhesive. It not only has the easy-to-operate process characteristics of ordinary hot melt adhesive, but also contains active isocyanate groups. It can still undergo curing and cross-linking reactions with moisture in the air at room temperature, thereby obtaining excellent bonding properties, good flexibility and weather resistance, etc. Therefore, it is widely used in consumer electronics, woodworking, home appliances, textiles and other industries.
[0003] Because the industry's environmental protection requirements are getting higher and higher, the adhesive needs to have the performance of being able to be disassembled at any time like screws. Due to the particularity of electronic products, the bonding strength cannot be destroyed at very high temperatures, making the adhesive easy to disassemble. Therefore, developing an easy-to-disassemble polyurethane hot melt adhesive is an urgent problem that needs to be solved. Summary of the invention
[0004] To achieve the above objectives, the present invention provides a disassembled polyurethane hot melt adhesive, the product of which can be easily disassembled under UV light conditions.
[0005] The technical solution of the present invention to solve the above technical problems is as follows: In parts by mass, the polyol polymer comprises 20-80 parts, the polyisocyanate compound comprises 5-40 parts, the modified resin comprises 0.1-5 parts, the thermoplastic resin comprises 1-30 parts, the tackifying resin comprises 1-12 parts, the photoinitiator comprises 0.01-10 parts, the thermal conductive filler comprises 10-60 parts, and the latent curing agent comprises 0.01-10 parts.
[0006] Described modified resin synthesis scheme: Add an appropriate amount of isocyanate to the reaction bottle, heat it to 60-80°C, add an appropriate amount of hydroxy alicyclic epoxy resin, heat it to 80-120°C, react for 30-90 minutes, add an appropriate amount of dehydrating agent to obtain a modified resin.
[0007] The isocyanate is a multifunctional isocyanate compound with a functionality of ≥3, and the hydroxy alicyclic epoxy resin is a monofunctional hydroxyl and multifunctional epoxy alicyclic epoxy resin compound; The molar ratio of the isocyanate to the hydroxy alicyclic epoxy resin is preferably 3:1; The dehydrating agent is a substance that can react with water, and is preferably a monofunctional isocyanate compound.
[0008] Synthesis scheme of polyurethane hot melt adhesive: Heat the polyol polymer, thermoplastic resin, tackifying resin, and thermal conductive filler to 120-140°C to remove water; Cool down to 80-100°C, continue to add appropriate amount of polyisocyanate compound, react for 30-90 minutes; add modified resin, latent curing agent, photoinitiator, stir evenly, discharge, and seal for storage.
[0009] The polyisocyanate compound is one or a mixture of methylene diphenyl diisocyanate (MDI), hydrogenated methylene diphenyl diisocyanate (HMDI), hexamethylene diisocyanate (HDI), isophorone diisocyanate (IPDI), polymerized methylene diphenyl diisocyanate, toluene diisocyanate (TDI), polymethylene polyphenyl diisocyanate, naphthalene diisocyanate (NDI) or polymethylene polyphenyl isocyanate (PAPI).
[0010] The molecular weight of the polyol polymer is 300-8000; The polyol polymer refers to a compound containing hydroxyl functionality, and may include polyester polyol polymers, polyether polyol polymers, or a mixture of several thereof.
[0011] The polyester polyol polymer includes common polyester polyol polymer, polycaprolactone polyol polymer and polycarbonate polyol polymer.
[0012] The common polyester polyol polymer is a polymer produced by the reaction of an acid or anhydride with a corresponding alcohol, and is polymerized by at least one of adipic acid, sebacic acid, dodecanoic acid, isophthalic acid, terephthalic acid, phthalic acid, phthalic anhydride and at least one of 1,4-butanediol, diethylene glycol, neopentyl glycol, ethylene glycol, cyclohexanediol, diethylene glycol, 1,6-hexanediol and 3-methyl-1,5-pentanediol.
[0013] The polycaprolactone polyol polymer is a poly-ε-caprolactone polyol obtained by ring-opening polymerization of ε-caprolactone.
[0014] The polycarbonate polyol polymer is a polymer containing a polycarbonate group, such as one or more of polycarbonate 1,6-hexanediol polyol, copolymerized polyesters such as pentanediol, hexanediol, butanediol, and propylene glycol, and polycyclohexane carbonate glycol polyol.
[0015] The polyether polyol polymer is a ring-opening polymer of ethylene glycol, propylene glycol, tetrahydrofuran, 3-methyltetrahydrofuran, and a random copolymer or block copolymer of them or their derivatives.
[0016] The thermoplastic resin is thermoplastic acrylic resin.
[0017] The tackifying resin is one or a mixture of terpene resin, rosin resin and petroleum resin.
[0018] The photoinitiator is a cationic epoxy curing photoinitiator, including diazonium salts, diaryl iodonium salts, triaryl sulfonium salts, alkyl sulfonium salts, iron arene salts, sulfonyloxy ketones and triaryl siloxane ethers. The latent curing agent is a compound that can be hydrolyzed to generate amines, and an oxazolidine latent curing agent may be mentioned.
[0019] The thermally conductive filler is a filler with a thermally conductive effect, including aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, silicon carbide, etc.
[0020] The beneficial effects of the present invention are: The alicyclic epoxy resin is grafted into the polyurethane system. The performance of the polyurethane itself is not affected during moisture curing. Under UV light, the alicyclic epoxy undergoes polymerization reaction, which improves the strength of the colloid body and reduces the peel strength. At the same time, the reaction generates heat, and the heat is transferred by adding thermal conductive materials, so that the colloid interface is heated evenly, the colloid temperature rises, the strength decreases, and it is easier to disassemble. DETAILED DESCRIPTION
[0021] Modified resin synthesis: Add an appropriate amount of isocyanate to the reaction bottle, heat it to 80°C, add an appropriate amount of hydroxy alicyclic epoxy resin, add it in molar equivalent (n(nco):n(-oH)=3:1), heat it to 100°C, react for 60 minutes, add an appropriate amount of dehydrating agent to obtain a modified resin.
[0022] Polyurethane hot melt adhesive synthesis: Step 1: Heat 20-80 parts of polyol polymer, 10-60 parts of aluminum oxide, 1-30 parts of thermoplastic resin, and 1-12 parts of tackifying resin to 120-140° C., and vacuum dehydrate for 2 hours at 300 r / min stirring; Step 2: Cool down to 100°C, continue to add 5-40 parts of polyisocyanate compound, react at a stirring speed of 400r / min under vacuum conditions for 1h, add 0.1-5 parts of modified resin, 0.01-10 parts of latent curing agent, and 0.01-10 parts of photoinitiator, stir for 30min under vacuum conditions, then discharge the material, vacuum seal and store away from light.
[0023] Example 1 By weight, 15 parts of polybutylene adipate polyol with a molecular weight of 2000, 12 parts of polyoxypropylene glycol with a molecular weight of 1000, 4 parts of polyhexylene phthalate glycol with a molecular weight of 1000, 7 parts of polyacrylic resin BR113, 4 parts of petroleum resin, and 40 parts of alumina were added to a reaction bottle, heated to 130-140°C, and vacuum dehydrated for 2 hours under a stirring condition of 350r / min. Then, the temperature was lowered to 100°C, 12 parts of 4,4'-diphenylmethane diisocyanate (MDI) were added, and after reacting for 1 hour at a stirring speed of 450r / min under vacuum conditions, 3 parts of modified resin were added, 3 parts of latent curing agent, and 0.1 parts of diaryliodonium salt were added, and the material was discharged after continuing to stir for 30 minutes, and vacuum sealed and stored in the dark.
[0024] Example 2 By weight, 14 parts of 2000 molecular weight polyhexane adipate polyol, 10 parts of 2000 molecular weight polytetrahydrofuran, 5 parts of 1000 molecular weight polyneopentyl adipate diol, 6 parts of polyacrylic resin BR113, 1 part of petroleum resin, and 45 parts of alumina were added to a reaction bottle, heated to 120-140°C, and vacuum dehydrated for 2 hours at 350r / min stirring. Then, the temperature was lowered to 100°C, 13 parts of 4,4-diisocyanate dicyclohexylmethane (HMDI) were added, and after reacting for 1 hour at a stirring speed of 450r / min under vacuum conditions, 3 parts of modified resin, 3 parts of latent curing agent, and 0.12 parts of diaryliodonium salt were added, and the mixture was stirred for 30 minutes before discharging, and vacuum sealed and stored in a dark place.
[0025] Example 3 By weight, 9 parts of 3500 molecular weight polyhexane adipate diol, 12 parts of 2000 molecular weight polycaprolactone diol, 8 parts of 1000 molecular weight polycarbonate diol, 2 parts of polyacrylic resin BR113, 2 parts of petroleum resin, and 50 parts of alumina were added to the reaction bottle, heated to 120-140°C, and vacuum dehydrated for 2 hours at 350r / min stirring. Then, the temperature was lowered to 100°C, 9 parts of 4,4'-diphenylmethane diisocyanate (MDI) were added, and the reaction was carried out at a stirring speed of 450r / min under vacuum conditions for 1 hour, and then 5 parts of modified resin, 3 parts of latent curing agent, and 0.12 parts of diaryliodonium salt were added, and the mixture was stirred for 30 minutes before discharging, vacuum sealing and light protection. Comparative Example Ordinary reactive polyurethane hot melt adhesive: by weight, add 24 parts of 3500 molecular weight polyhexane adipate diol, 20 parts of 2000 molecular weight polyneopentyl adipate diol, 23 parts of 2000 molecular weight polytetrahydrofuran ether diol, and 18 parts of acrylic resin BR113 to the reaction bottle, heat to 130-140°C, and vacuum dehydrate for 2 hours under 300 / min stirring conditions. Then, cool to 100°C, add 14.9 parts of 4,4'-diphenylmethane diisocyanate (MDI), react for 1 hour under vacuum conditions at a stirring speed of 450r / min, stir for 30 minutes under vacuum conditions at a stirring speed of 450r / min, then discharge, vacuum seal and store in a dark place.
[0026] The performance test results of the products obtained in Examples 1-3 and Comparative Examples are shown in Table 1.
[0027] Apply polyurethane hot melt adhesive to the glass plate, let it cure for 72 hours, then expose it to UV light for 365 days to test the immediate bonding strength.
[0028] The polyurethane hot melt adhesive was made into a film, cured for 72 hours, and then irradiated with a UV lamp for 365 days, and then the body strength of the film was tested.
[0029]
[0030] From the comparative data, it can be seen that the polyurethane hot melt adhesive prepared by the present invention has lower bonding strength and higher body strength after being cured and irradiated with ultraviolet light, and is therefore easier to disassemble.
[0031] The above description is only a preferred embodiment of the present invention and is not intended to limit the present invention. Any modifications, equivalent substitutions, improvements, etc. made within the spirit and principle of the present invention should be included in the protection scope of the present invention.
Claims
1. A disassembled polyurethane hot melt adhesive, which comprises, by weight, 20-80 parts of a polyol polymer, 5-40 parts of a polyisocyanate compound, 0.1-5 parts of a modified resin, 1-30 parts of a thermoplastic resin, 1-12 parts of a tackifying resin, 0.01-10 parts of a photoinitiator, 10-60 parts of a thermally conductive filler, and 0.01-10 parts of a latent curing agent.
2. The demountable polyurethane hot melt adhesive according to claim 1, characterized in that: The modified resin synthesis scheme is as follows: adding an appropriate amount of isocyanate to a reaction bottle, heating to 60-80°C, adding an appropriate amount of hydroxy alicyclic epoxy resin, heating to 80-120°C, reacting for 30-90 minutes, and then adding an appropriate amount of dehydrating agent to obtain a modified resin; the isocyanate is a multifunctional isocyanate compound with a functionality of ≥3; the hydroxy alicyclic epoxy resin is a monofunctional hydroxyl and multifunctional epoxy alicyclic epoxy resin compound; the molar ratio of the isocyanate to the hydroxy alicyclic epoxy resin is 3:1; and the dehydrating agent is a monofunctional isocyanate compound.
3. The demountable polyurethane hot melt adhesive according to claim 1, characterized in that: The polyol polymer is a mixture of one or more polyester polyol polymers and polyether polyol polymers containing hydroxyl functionality and a molecular weight of 300-8000; the polyisocyanate compound is one or more of methylene diphenyl diisocyanate, hydrogenated methylene diphenyl isocyanate, hexamethylene diisocyanate, isophorone diisocyanate, polymerized methylene diphenyl diisocyanate, toluene diisocyanate, polymethylene polyphenyl diisocyanate, naphthalene diisocyanate or polymethylene polyphenyl isocyanate.
4. The demountable polyurethane hot melt adhesive according to claim 3, characterized in that: The polyester polyol polymer includes common polyester polyol polymer, polycaprolactone polyol polymer and polycarbonate polyol polymer; the common polyester polyol polymer is a polymer produced by the reaction of an acid or anhydride with a corresponding alcohol, and is polymerized by at least one of adipic acid, sebacic acid, dodecanoic acid, isophthalic acid, terephthalic acid, phthalic acid, phthalic anhydride and 1,4-butanediol, diethylene glycol, neopentyl glycol, ethylene glycol, cyclohexanediol, diethylene glycol, 1,6-hexanediol and 3-methyl-1,5-pentanediol; the polycaprolactone polyol polymer is a poly-ε-caprolactone polyol obtained by ring-opening polymerization of ε-caprolactone; the polycarbonate polyol polymer is a polymer containing a polycarbonate group; the polyether polyol polymer is a ring-opening polymer of ethylene glycol, propylene glycol, tetrahydrofuran, 3-methyltetrahydrofuran, and a random copolymer or block copolymer of them or their derivatives.
5. The demountable polyurethane hot melt adhesive according to claim 1, characterized in that: The thermoplastic resin is a thermoplastic acrylic resin; the tackifying resin is one or a mixture of terpene resin, rosin resin, and petroleum resin; the photoinitiator is one of diazonium salt, diaryl iodonium salt, triaryl sulfonium salt, alkyl sulfonium salt, iron aromatic salt, sulfonyloxy ketone, and triaryl siloxane; the latent curing agent is an oxazolidine latent curing agent; and the thermal conductive filler is one or more of aluminum oxide, magnesium oxide, zinc oxide, aluminum nitride, boron nitride, and silicon carbide.
6. The decomposable polyurethane hot melt adhesive according to claim 1, wherein the synthesis scheme is as follows: Heat the polyol polymer, thermoplastic resin, tackifying resin, and thermal conductive filler to 120-140°C to remove water; Cool down to 80-100℃, continue to add appropriate amount of polyisocyanate compound, and react for 30-90min; Add modified resin, latent curing agent and photoinitiator, stir evenly, discharge the material and seal for storage.
Citation Information
Patent Citations
Hardenable resin composition
CN101193975A
Preparation method of ultraviolet light curing composite binding agent
CN101798492A
A modified polyurethane material for bridge expansion joints and its preparation method
CN114933884A
Epoxy modified low-VOC (volatile organic compound) two-component polyurethane adhesive and preparation method thereof
CN116162434A
Modified polyurethane hot melt adhesive with high initial adhesion and temperature resistance as well as preparation method and application of modified polyurethane hot melt adhesive
CN116656303A