Heat treatment process of DH36 steel plate

A multi-stage heat treatment process for DH36 steel plates addresses the challenge of achieving desired strength ratios and uniformity by refining grain structure and controlling cooling methods, resulting in improved mechanical properties and avoiding overcooling.

CN119082425APending Publication Date: 2024-12-06HEBEI PUYANG IRON & STEEL
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411228047.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-03
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

Existing heat treatment processes for DH36 steel plates struggle to achieve yield strength of ≥400MPa and yield strength ratio ≤0.85 without inducing overcooling structures, which compromise the uniformity and performance of the steel.

Method used

A multi-stage heat treatment process involving first heating, annealing, second heating, and controlled oil quenching to refine grain structure, eliminate defects, and adjust mechanical properties, including specific temperature and time controls to prevent overcooling.

Benefits of technology

The process achieves DH36 steel plates with yield strength ≥400MPa and yield strength ratio ≤0.85, ensuring uniform mechanical properties and avoiding overcooling structures, thereby enhancing plasticity, toughness, and overall performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082425A_ABST
    Figure CN119082425A_ABST
Patent Text Reader

Abstract

The invention provides a heat treatment process of a DH36 steel plate, and belongs to the technical field of steel processing. Through the first heating treatment, the structure of the steel is more uniform, grains are refined, the structure defects are eliminated, and the plasticity and toughness of the material are further improved; the residual stress of the steel is reduced through annealing treatment, the size is stabilized, the deformation and crack tendency is reduced, preparation is made for subsequent further treatment, the temperature difference of the test piece is reduced through second heating treatment and heat preservation for a certain time, phase change is evenly conducted on the whole section of the test piece, and large structural stress can be avoided; austenite nucleation, growth, carbide dissolution, component homogenization and diffusion migration of alloy elements are promoted by controlling the heat preservation temperature and the heat preservation time after the third heating treatment, then first oil quenching cooling is conducted, the grain size is controlled to make structural preparation for subsequent second oil quenching cooling, the obdurability matching of the steel plate can be adjusted, and the strength and toughness of the steel plate can be adjusted. And the DH36 steel plate with good comprehensive mechanical properties is obtained.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of steel processing, and in particular to a heat treatment process for a DH36 steel plate. Background Art

[0002] The chemical composition of DH36 steel plate mainly includes carbon, manganese, silicon, phosphorus, sulfur and other elements. Among them, carbon is one of the important elements that affect the strength and toughness of steel plate. Manganese and silicon can improve the strength and hardness of steel plate, while phosphorus and sulfur have a negative impact on the plasticity and toughness of steel plate. DH36 steel plate is a high-performance steel. Compared with other steels, DH36 steel has higher strength and toughness, can withstand greater loads and impact forces, and its excellent welding performance also makes construction more convenient and quick. DH36 steel also has good corrosion resistance and weather resistance, which can greatly extend the service life of the project. Among them, DH36 steel plate has high yield strength and tensile strength, which makes it perform well when subjected to heavy loads and complex stresses, and can effectively ensure the stability of the hull and other structures. Therefore, DH36 steel plate has been widely used in marine engineering, shipbuilding, bridge construction, petrochemical, electric power and construction. In marine engineering, DH36 steel plates are used to build offshore platforms, submarine pipelines, offshore drilling platforms and other structures; in shipbuilding, DH36 steel plates are mainly used to manufacture hull structures, decks, bulkheads and other components; in bridge construction, DH36 steel plates are used to build bridge main beams, cross beams, bridge decks and other parts. In addition, DH36 steel plates are also widely used in petrochemical, electric power and construction fields, such as the construction of refining equipment, storage tanks, power generation equipment, transmission towers and other structural parts.

[0003] The production process of DH36 steel plate includes steelmaking, rolling, heat treatment and other links. In the steelmaking process, the chemical composition and temperature control need to be strictly controlled to ensure the quality and performance of the steel plate. In the rolling process, through reasonable rolling process and rolling temperature, the steel plate has good organizational structure and mechanical properties. In the heat treatment process, by controlling parameters such as heating temperature, holding time and cooling rate, the mechanical properties and corrosion resistance of the steel plate are further improved.

[0004] With the advancement of technology, the market has higher and higher performance requirements for DH36 steel plates, requiring the yield strength of DH36 steel plates to be ≥400Mpa and the yield strength ratio to be ≤0.85. At the same time, in order to ensure that the performance of the steel plate is uniform and does not affect processing, overcooling structure is not allowed. However, in actual production, in order to ensure that this strength is achieved, water cooling must be assisted after normalizing, but water cooling cannot avoid the appearance of overcooling structure. Therefore, providing a heat treatment process for DH36 steel plates that better meets market demand is a technical problem that the existing technology urgently needs to solve. Summary of the invention

[0005] The object of the present invention is to provide a heat treatment process for a DH36 steel plate. By the heat treatment process provided by the present invention, the yield strength of the DH36 steel plate obtained is not less than 400Mpa, the yield strength ratio is not greater than 0.85, and at the same time, there is no supercooled structure on the surface of the obtained DH36 steel plate.

[0006] In order to achieve the above-mentioned object of the invention, the present invention provides the following technical solutions:

[0007] The present invention provides a heat treatment process for a DH36 steel plate, comprising the following steps:

[0008] The DH36 steel plate to be treated is subjected to a first heating treatment and heated to 910-920°C, kept at this temperature for 1.3-2 min / mm, and then cooled to room temperature along with the furnace to obtain an annealed steel plate;

[0009] The annealed steel plate is subjected to a second heat treatment to raise the temperature to 600-730°C, and kept warm for 1.5-2 min / mm, and then subjected to a third heat treatment to raise the temperature to 900-910°C, and kept warm for 2-3 min / mm, and then subjected to a first oil quenching to cool to 600-730°C, and kept warm for 1.1-1.6 min / mm, and then subjected to a second oil quenching to cool to room temperature.

[0010] Preferably, the first heating treatment is performed by heating the temperature to 910-920° C. within 3-5 hours.

[0011] Preferably, the holding time after the first heat treatment is 1.5 to 1.8 min / mm.

[0012] Preferably, the second heating treatment is performed by heating the temperature to 600-730° C. within 2-4 hours.

[0013] Preferably, the holding time after the second heat treatment is 1.6 to 1.8 min / mm.

[0014] Preferably, the holding time after the third heat treatment is 2.6 to 2.8 min / mm.

[0015] Preferably, the temperature of the oil used in the first oil quenching is 20-30°C.

[0016] Preferably, after the first oil quenching cooling, the temperature is kept at 1.2 to 1.4 min / mm.

[0017] Preferably, the chemical composition and mass percentage of the DH36 steel plate to be treated are: C: 0.08% to 0.12%; Si: 0.20% to 0.32%; Mn: 1.35% to 1.50%; P≤0.015%; S≤0.005%; Als: 0.020% to 0.050%; Nb: 0.028% to 0.040%; Cu: 0.15% to 0.20%; V: 0.040% to 0.060%; Ti: 0.008% to 0.018%, and the rest are Fe and unavoidable impurities.

[0018] Preferably, the DH36 steel plate to be processed has a thickness of 90 to 110 mm and a width of 1500 to 2600 mm.

[0019] The invention provides a heat treatment process for a DH36 steel plate. The first heating treatment makes the structure of the steel more uniform, refines the grains, eliminates the structural defects, and further improves the plasticity and toughness of the material. The annealing treatment can also reduce the residual stress of the steel, stabilize the size, reduce the tendency of deformation and cracking, and prepare for subsequent further treatment. The second heating treatment is used and the heat preservation is performed for a certain time to reduce the temperature difference of the test piece, prepare for phase change, and make the phase change uniformly performed on the entire cross section of the test piece, thereby avoiding the generation of large structural stress. Then, the heat preservation temperature and the heat preservation time after the third heating treatment are controlled to promote austenite nucleation, growth, dissolution of carbides and homogenization of components, and diffusion and migration of alloy elements. Then, the first oil quenching cooling is performed to control the grain size to prepare for the structure for the subsequent second oil quenching cooling. The strength and toughness of the steel plate can be adjusted, and the appearance of the overcooled structure can be avoided, so as to obtain the DH36 steel plate with good comprehensive mechanical properties. BRIEF DESCRIPTION OF THE DRAWINGS

[0020] Figure 1 This is a bar chart comparing some mechanical properties of DH36 steel plates prepared in Examples 1 to 3 of the present invention and Comparative Examples 1 to 3. DETAILED DESCRIPTION

[0021] The present invention provides a heat treatment process for a DH36 steel plate, comprising the following steps:

[0022] The DH36 steel plate to be treated is subjected to a first heating treatment and heated to 910-920°C, kept at this temperature for 1.3-2 min / mm, and then cooled to room temperature along with the furnace to obtain an annealed steel plate;

[0023] The annealed steel plate is subjected to a second heat treatment to raise the temperature to 600-730°C, and kept warm for 1.5-2 min / mm, and then subjected to a third heat treatment to raise the temperature to 900-910°C, and kept warm for 2-3 min / mm, and then subjected to a first oil quenching to cool to 600-730°C, and kept warm for 1.1-1.6 min / mm, and then subjected to a second oil quenching to cool to room temperature.

[0024] In one embodiment, the first heating treatment is performed by heating the temperature to 910-920° C. within 3-5 hours.

[0025] In one embodiment, the first heating treatment is performed by heating the temperature to 910-920° C. within 4 hours.

[0026] In one embodiment, the holding time after the first heat treatment is 1.5 to 1.8 min / mm.

[0027] The main purpose of annealing is to reduce the hardness of steel, so as to reduce the hardness of steel and improve its processability. The present invention can make the structure of steel more uniform, refine grains, eliminate structural defects, and further improve the plasticity and toughness of materials by controlling the holding temperature and holding time of the first heating treatment; annealing can also reduce the residual stress of steel, stabilize the size, reduce deformation and crack tendency, and improve the dimensional stability and durability of steel, and by controlling the heating time, holding temperature and holding time of the first heating treatment, the microstructure of steel can be optimized, thereby improving its mechanical properties and processing performance.

[0028] In one embodiment, the second heating treatment is performed by heating the temperature to 600-730° C. within 2-4 hours.

[0029] In one embodiment, the second heat treatment is performed by heating the temperature to 600-730° C. within 3 hours.

[0030] In one embodiment, the holding time after the second heat treatment is 1.6 to 1.8 min / mm.

[0031] In one embodiment, the third heat treatment is performed by heating the temperature to 600-730° C. within 1-2 hours.

[0032] In one embodiment, the holding time after the third heat treatment is 2.6 to 2.8 min / mm.

[0033] The present invention first performs a second heating treatment and holds the heat for a certain period of time to reduce the temperature difference of the test piece, prepare for phase transformation, and make the phase transformation evenly carried out on the entire cross section of the test piece, thereby avoiding the generation of large tissue stress. Then, the holding temperature and holding time after the third heating treatment are controlled to promote austenite nucleation, growth, dissolution of carbides and homogenization of components, and diffusion and migration of alloy elements. Then, the first oil quenching is performed to control the grain size to prepare the tissue for the subsequent second oil quenching, and the strength and toughness combination of the steel plate can be adjusted to obtain a DH36 steel plate with good comprehensive mechanical properties.

[0034] In one embodiment, the temperature of the oil used in the first oil quenching is 20-30°C.

[0035] In one embodiment, after the first oil quenching, the temperature is kept at 1.2 to 1.4 min / mm.

[0036] In one embodiment, the temperature of the oil used in the second oil quenching is 20-30°C.

[0037] The present invention utilizes the first oil quenching cooling and the second oil quenching cooling to adjust the cooling speed, avoid cracking of the test piece and reduce deformation, and avoid the appearance of overcooling structure, so as to prepare a DH36 steel plate with good comprehensive mechanical properties.

[0038] In one embodiment, the chemical composition and mass percentage of the DH36 steel plate to be treated are: C: 0.08% to 0.12%; Si: 0.20% to 0.32%; Mn: 1.35% to 1.50%; P≤0.015%; S≤0.005%; Als: 0.020% to 0.050%; Nb: 0.028% to 0.040%; Cu: 0.15% to 0.20%; V: 0.040% to 0.060%; Ti: 0.008% to 0.018%, and the rest is Fe and unavoidable impurities.

[0039] In one embodiment, the DH36 steel plate to be processed has a thickness of 90 to 110 mm and a width of 1500 to 2600 mm.

[0040] In one embodiment, the DH36 steel plate to be processed has a thickness of 95 to 105 mm and a width of 1600 to 2200 mm.

[0041] The technical solutions in the present invention will be described clearly and completely below in conjunction with the embodiments of the present invention. Obviously, the described embodiments are only a part of the embodiments of the present invention, not all of them. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work are within the scope of protection of the present invention.

[0042] Example 1

[0043] A heat treatment process for DH36 steel plate, the steps are as follows:

[0044] The chemical composition and mass percentage of the DH36 steel plate to be treated are: C: 0.08%; Si: 0.22%; Mn: 1.38%; P≤0.015%; S≤0.005%; Als: 0.030%; Nb: 0.038%; Cu: 0.18%; V: 0.056%; Ti: 0.015%, and the rest is Fe and unavoidable impurities;

[0045] The DH36 steel plate to be processed has a thickness of 90 mm and a width of 1600 mm;

[0046] The DH36 steel plate to be treated is subjected to a first heating treatment by heating the temperature to 910°C within 4 hours, keeping the temperature for 1.5 min / mm, and then cooling the temperature to room temperature with the furnace to obtain an annealed steel plate;

[0047] The annealed steel plate is subjected to a second heat treatment to raise the temperature to 680°C within 3 hours, and is kept warm for 1.7 min / mm, and then subjected to a third heat treatment to raise the temperature to 900°C, and is kept warm for 2.6 min / mm, and then is cooled to 630°C through a first oil quenching, and is kept warm for 1.3 min / mm, and then is cooled to room temperature through a second oil quenching.

[0048] Example 2

[0049] The DH36 steel plate was heat treated according to the method of Example 1, except that the annealed steel plate was subjected to a second heating treatment to raise the temperature to 690° C. within 3 hours.

[0050] Example 3

[0051] The DH36 steel plate was subjected to a heat treatment process according to the method of Example 1, except that the annealed steel plate was subjected to a second heating treatment to raise the temperature to 720° C. within 3 hours.

[0052] Comparative Example 1

[0053] The DH36 steel plate is heat treated according to the method of Example 1, except that the first heating treatment is not performed and the second heating treatment is directly performed.

[0054] Comparative Example 2

[0055] The DH36 steel plate is heat treated according to the method of Example 1, except that the second heat treatment is not performed and the third heat treatment is performed directly.

[0056] Comparative Example 3

[0057] The DH36 steel plate was heat treated according to the method of Example 1, except that the first oil quenching and the second oil quenching were respectively modified to the first water quenching and the second water quenching.

[0058] The mechanical properties of the DH36 steel plates prepared in Examples 1 to 3 and Comparative Examples 1 to 3 were tested. The results are shown in Table 1. The bar graphs of some mechanical properties are shown in Table 1. Figure 1 shown.

[0059] Table 1 Mechanical properties statistics of DH36 steel plates prepared in Examples 1 to 3 and Comparative Examples 1 to 3

[0060]

[0061]

[0062] From Table 1 and Figure 1 It can be seen that the yield strength of the DH36 steel plates after heat treatment in Examples 1 to 3 of the present invention can reach 490 MPa, the tensile strength can reach 601 MPa, the yield strength is not less than 400 MPa, and the yield strength ratio is not greater than 0.85.

[0063] Example 4

[0064] A heat treatment process for DH36 steel plate, the steps are as follows:

[0065] The chemical composition and mass percentage of the DH36 steel plate to be treated are: C: 0.10%; Si: 0.20%; Mn: 1.35%; P≤0.015%; S≤0.005%; Als: 0.025%; Nb: 0.032%; Cu: 0.16%; V: 0.050%; Ti: 0.010%, and the rest is Fe and unavoidable impurities;

[0066] The DH36 steel plate to be processed has a thickness of 90 mm and a width of 1600 mm;

[0067] The DH36 steel plate to be treated is subjected to a first heating treatment by heating the temperature to 920°C within 4 hours, keeping the temperature for 1.5 min / mm, and then cooling the temperature to room temperature with the furnace to obtain an annealed steel plate;

[0068] The annealed steel plate is subjected to a second heat treatment to raise the temperature to 700°C within 3 hours and keep it warm for 1.7 min / mm, then subjected to a third heat treatment to raise the temperature to 905°C and keep it warm for 2.6 min / mm, then subjected to a first oil quenching to cool to 660°C and keep it warm for 1.3 min / mm, and then subjected to a second oil quenching to cool to room temperature.

[0069] Example 5

[0070] The DH36 steel plate was heat treated according to the method of Example 4, except that the annealed steel plate was subjected to a second heating treatment to raise the temperature to 720°C within 3 hours.

[0071] Example 6

[0072] The DH36 steel plate was subjected to a heat treatment process according to the method of Example 4, except that the annealed steel plate was subjected to a second heating treatment to raise the temperature to 730° C. within 3 hours.

[0073] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.

Claims

1. A heat treatment process for DH36 steel plate, characterized in that: The following steps are involved: The DH36 steel plate to be treated is subjected to a first heating treatment and heated to 910-920°C, kept at this temperature for 1.3-2 min / mm, and then cooled to room temperature along with the furnace to obtain an annealed steel plate; The annealed steel plate is subjected to a second heat treatment to raise the temperature to 600-730°C, and kept warm for 1.5-2 min / mm, and then subjected to a third heat treatment to raise the temperature to 900-910°C, and kept warm for 2-3 min / mm, and then subjected to a first oil quenching to cool to 600-730°C, and kept warm for 1.1-1.6 min / mm, and then subjected to a second oil quenching to cool to room temperature.

2. The heat treatment process according to claim 1, characterized in that: The first heating treatment is performed by heating the temperature to 910-920° C. within 3-5 hours.

3. The heat treatment process according to claim 1, characterized in that: The heat preservation time after the first heat treatment is 1.5 to 1.8 min / mm.

4. The heat treatment process according to claim 1, characterized in that: The second heating treatment is performed by heating the temperature to 600-730° C. within 2-4 hours.

5. The heat treatment process according to claim 1, characterized in that: The heat preservation time after the second heat treatment is 1.6 to 1.8 min / mm.

6. The heat treatment process according to claim 1, characterized in that: The heat preservation time after the third heat treatment is 2.6 to 2.8 min / mm.

7. The heat treatment process according to claim 1, characterized in that: The temperature of the oil used in the first oil quenching is 20-30°C.

8. The heat treatment process according to claim 1, characterized in that: The holding time after the first oil quenching is 1.2 to 1.4 min / mm.

9. The heat treatment process according to claim 1, characterized in that: The chemical composition and mass percentage of the DH36 steel plate to be treated are: C: 0.08% to 0.12%; Si: 0.20% to 0.32%; Mn: 1.35% to 1.50%; P≤0.015%; S≤0.005%; Als: 0.020% to 0.050%; Nb: 0.028% to 0.040%; Cu: 0.15% to 0.20%; V: 0.040% to 0.060%; Ti: 0.008% to 0.018%, and the rest is Fe and unavoidable impurities.

10. The heat treatment process according to claim 1, characterized in that: The DH36 steel plate to be processed has a thickness of 90 to 110 mm and a width of 1500 to 2600 mm.