Refining method for resourceful treatment of zinc-containing material by combining pyrogenic process and wet process

Through the resource processing method combined with fire and wet method, the impurities in crude zinc oxide are removed, and the problems of high energy consumption and secondary pollution in traditional recycling technology are solved, and the high purity recycling of zinc and lead and lead-zinc are achieved. Separation achieves the recycling of zinc and lead with low energy consumption and no secondary pollution.

CN119082469APending Publication Date: 2024-12-06CHONGQING UNIVERSITY OF SCIENCE AND TECHNOLOGY
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411192873.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-28
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The traditional fire recovery technology of crude zinc oxide has problems of high energy consumption and secondary pollution, and the impurity content in crude zinc is high, which affects the recycling efficiency of zinc and lead.

Method used

Using the resource treatment method combined with fire and wet method, the impurities in crude zinc oxide are gradually removed through reducing calcination, oxidation and baking, acid dissolution, replacement and carbonate processes, and the recovery and purity of zinc and lead are improved. .

Benefits of technology

It realizes high purity recycling of zinc and lead with low energy consumption and no secondary pollution, improves the recovery rate of zinc and lead, and the entire process elements can be recycled and brine can be reused.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082469A_ABST
    Figure CN119082469A_ABST
Patent Text Reader

Abstract

The invention discloses a refining method for resourceful treatment of a zinc-containing material by combining a pyrogenic process and a wet process, which comprises the following steps: firstly, adding carbon, limestone, silica and bentonite into the zinc-containing material, uniformly mixing, performing reduction roasting under a high-temperature condition, and collecting coarse zinc oxide powder; carrying out oxidizing roasting on the coarse zinc oxide powder under a high-temperature condition, and collecting secondary zinc-containing dust and solid-phase high-purity zinc oxide; and finally, the secondary zinc-containing dust is sequentially subjected to acid dissolution, replacement and carbonation, and zinc and lead in the secondary zinc-containing dust are separated. The method has the remarkable effects that low-energy-consumption resourceful treatment can be carried out on the crude zinc oxide separated by the pyrogenic process, impurities in the crude zinc oxide are removed, the purity of the zinc element is improved, valuable metal elements in the crude zinc oxide are recycled, the technological process is convenient to operate, and secondary pollutants are avoided.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to a waste resource recovery technology, in particular to a zinc-containing waste resource recovery technology. Background Art

[0002] The steel smelting process produces a large amount of Zn-containing by-products such as blast furnace ash and electric furnace ash. These materials contain elements such as Zn, Pb, Fe, Cd, Sn, In, Cl, and F. Direct landfill will cause huge environmental pollution and waste of resources.

[0003] The source of Zn in blast furnace ash is: in the blast furnace ironmaking process, the main raw material used is iron ore, and the ore inevitably contains trace amounts of Zn (about 0.1%). After the ore is put into the blast furnace, Zn volatilizes (sublimates) into the flue gas system, is oxidized in the air and is collected by gravity dust removal bags at all levels in the form of ZnO dust, collectively referred to as blast furnace ash. The Zn content in blast furnace ash is usually around 5%.

[0004] The source of Zn in electric furnace ash is: electric furnace steelmaking uses scrap steel as the main raw material, especially Zn-plated automobile sheet scrap steel. After smelting in the electric furnace, Zn will volatilize to the flue gas dust collection system and be collected in the form of ZnO dust. The Zn content in electric furnace ash is usually around 20%.

[0005] The types and contents of specific elements in blast furnace ash and circuit ash from different batches and manufacturers vary, but are generally similar. Resource recycling plants generally mix a variety of Zn-containing dusts, which mainly contain 10-20% Zn and 25-40% Fe.

[0006] The traditional Zn resource process simply uses a rotary kiln or a rotary hearth furnace for reduction roasting (fire method) to prepare crude ZnO and Fe-rich materials. The crude ZnO is sold directly and can be used by downstream manufacturers to prepare electrolytic Zn. However, crude ZnO contains many impurities, and direct electrolysis generates high energy consumption and serious secondary pollution. Summary of the invention

[0007] The present invention provides a method for further low-energy resource treatment of crude ZnO separated by pyrometallurgy, so as to realize the recycling of various valuable metal elements in the crude ZnO. The main technical scheme adopted is:

[0008] A refining method for treating zinc-containing materials by combining pyrometallurgy and hydrometallurgy, the key is to follow the following steps:

[0009] Step 1: Add charcoal, limestone, silica and bentonite to the zinc-containing material, mix well and perform reduction roasting under high temperature conditions, collect the zinc element reduced to gaseous state and volatilized, and the zinc element is oxidized in the air after volatilization to obtain coarse zinc oxide powder; at the same time, iron element is also reduced, but iron element is relatively not easy to volatilize, so zinc and iron can be separated;

[0010] Step 2: oxidatively roasting the crude zinc oxide powder under high temperature conditions, collecting the volatilized secondary zinc-containing dust, and the remaining solid phase is high-purity zinc oxide;

[0011] Step 3, adding the secondary zinc-containing dust into excess dilute hydrochloric acid, mixing and slurrying, dissolving, precipitating and filtering to obtain a primary zinc-containing filtrate and a primary impurity precipitate;

[0012] Step 4: adding elemental zinc to the primary zinc-containing filtrate to carry out a replacement reaction, dissolving, precipitating and filtering to obtain a secondary zinc-containing filtrate and a secondary impurity precipitate;

[0013] Step 5, adding excess sodium carbonate to the secondary zinc-containing filtrate, dissolving, precipitating and filtering to obtain a tertiary impurity filtrate and a tertiary zinc-containing precipitate;

[0014] The zinc-containing precipitates are collected three times and subjected to a high temperature of more than 350°C to obtain zinc oxide.

[0015] The method of the present invention is based on the traditional pyrometallurgical recovery technology of crude zinc oxide, adding wet processes such as oxidation roasting, acid hydrolysis, replacement, carbonation, etc., so as to further remove impurities in the crude ZnO and improve the recovery rate and purity of ZnO and PbO.

[0016] The present invention utilizes the different sublimation temperatures and solubilities of each element / compound to remove impurities in ZnO. The relevant sublimation temperature, relevant reaction formula, solubility and other information belong to the well-known technology well known to those skilled in the art, and therefore do not need to be specifically explained.

[0017] In addition, in each step, the ratio of various substances does not need to be specifically limited; on the one hand, different manufacturers have different actual contents of zinc oxide when mixing ingredients, resulting in different amounts of subsequent materials; on the other hand, detecting the amount of zinc element in the secondary zinc-containing dust, the primary zinc-containing filtrate, and the secondary zinc-containing filtrate, and configuring the corresponding optimal ratio of related materials according to the amount of the substance is also a well-known technology familiar to those skilled in the art; on the third hand, even if those skilled in the art do not configure the optimal ratio of related materials according to the amount of zinc element, the method of the present invention can remove impurities in crude ZnO to a certain extent.

[0018] The invention is characterized by using a low-energy, non-secondary-pollution wet process to achieve the refining of crude zinc oxide and the extraction and preparation of high-purity PbO products, thus achieving "lead-zinc separation". All elements used in the whole process can be recycled, and the brine can be recycled. BRIEF DESCRIPTION OF THE DRAWINGS

[0019] Figure 1 is a flow chart of the present invention;

[0020] Figure 2 The XRD phase analysis results of the secondary zinc-containing dust in Example 2;

[0021] Figure 3 This is the XRD phase analysis result of the primary impurity precipitation in Example 2;

[0022] Figure 4 The XRD phase analysis results of the three zinc-containing precipitates in Example 2;

[0023] Figure 5 The XRD phase analysis results of the lead-containing precipitate and the salt solution dried product in Example 2 are shown. DETAILED DESCRIPTION

[0024] The present invention is further described below in conjunction with embodiments and drawings.

[0025] Embodiment 1:

[0026] like Figure 1 As shown, a refining method for resource-processing zinc-containing materials by combining pyrometallurgy and hydrometallurgy is carried out in the following steps:

[0027] Step 1, adding carbon, limestone, silica and bentonite to the zinc-containing material, mixing and then performing reduction roasting under high temperature conditions, the zinc-containing material contains elements such as Zn, Pb, Fe, Cd, Sn, In, Cl, F, etc., the roasting temperature should exceed the sublimation temperature of zinc, so that the zinc in the zinc-containing material is reduced to zinc, then gasified, volatilized and overflowed, collecting the zinc reduced to gaseous state and volatilized, the zinc is easily oxidized in the air, and the crude zinc oxide powder is obtained;

[0028] Step 2: oxidatively roasting the coarse zinc oxide powder under high temperature conditions. The roasting temperature is higher than the sublimation temperature of the impurities to be removed but lower than the sublimation temperature of zinc oxide. The impurities are vaporized and volatilized. At the same time, some zinc oxide dust may also float out. The volatilized dust is collected, which contains a small amount of zinc oxide. The dust at this time is called secondary zinc-containing dust, and the remaining solid phase is high-purity zinc oxide.

[0029] Step 3: adding the secondary zinc-containing dust into excess dilute hydrochloric acid and mixing to make pulp. The purpose of adding excess dilute hydrochloric acid is to fully dissolve zinc oxide to obtain zinc chloride, and chloride salt solutions of other impurities may be generated during the process; after full dissolution, precipitation and filtration, a primary zinc-containing filtrate and a primary impurity precipitate are obtained;

[0030] Step 4: adding elemental zinc to the primary zinc-containing filtrate to carry out a replacement reaction, dissolving, precipitating, and filtering to obtain a secondary zinc-containing filtrate and a secondary impurity precipitate;

[0031] Step 5, adding excess sodium carbonate to the secondary zinc-containing filtrate, dissolving, precipitating and filtering to obtain a tertiary impurity filtrate and a tertiary zinc-containing precipitate;

[0032] The zinc-containing precipitates are collected three times and treated at a high temperature above 350°C to obtain high-purity zinc oxide.

[0033] Embodiment 2:

[0034] like Figure 1 As shown, a refining method for resource-processing zinc-containing materials by combining pyrometallurgy and hydrometallurgy is carried out in the following steps:

[0035] Step 1: Add carbon, limestone, silica and bentonite to the zinc-containing material, mix well and then perform reduction roasting under high temperature conditions; the zinc-containing material is a mixture of blast furnace ash and electric furnace ash, wherein the content of each element in a certain batch of blast furnace ash and electric furnace ash is shown in Table 1:

[0036] Table 1. Element content in blast furnace ash and electric furnace ash (wt%)

[0037] Material Name Zn Fe Pb Ca Si Na K Cl Sn Cd Cu S F Blast furnace ash 5.8 32.5 0.2 17.1 3.4 0.5 0.2 0.4 - - - - - Electric furnace ash 19.8 25.9 1.0 2.1 7.7 2.4 3.2 4.1 - - - - -

[0038] Zinc-containing materials contain elements such as Zn, Fe, Pb, Cl, etc., while the content of elements such as Cd, Sn, In, F, etc. is extremely low, but not zero (represented as "-").

[0039] Using Table 2 as a guide, blast furnace ash and electric furnace ash are batched to obtain zinc-containing materials:

[0040] Table 2. Element content of zinc-containing materials (wt%)

[0041]

[0042] In a mixture of zinc-containing material, charcoal, limestone, silica and bentonite, the mass percentage of charcoal is 15-35%, the mass percentage of limestone is 2-8%, the mass percentage of silica is ≤5%, and the mass percentage of bentonite is ≤2%;

[0043] The temperature-time of reduction roasting is: using a rotary kiln, a rotary hearth furnace or a vertical furnace to raise the temperature to 1100-1350°C within 100-150 minutes, and maintaining it for 15-80 minutes, collecting the zinc element that is reduced to gaseous state and volatilized between 1100-1350°C, and the zinc element is easily oxidized in the air to obtain a crude zinc oxide powder, which contains a variety of impurities such as Pb, Cl, K, etc., and the purity of the zinc element is usually only 50%-60%;

[0044] As the volatile substances in the zinc-containing material are separated, the Fe2O3 in the Fe is also reduced to form elemental Fe. Some of the elemental Fe may be oxidized during the cooling process. The obtained Fe product is called reduced Fe material and can be used as Fe-rich fine powder.

[0045] Step 2, the crude zinc oxide powder is aerobically roasted at 800-1150° C. for 15-80 min. In this process, natural gas heating or electric thermocouple heating can be used to create a high-temperature oxidizing atmosphere, and the volatiles can be blown out with appropriate airflow. Some zinc oxide dust may also float out, and the secondary zinc-containing dust that is volatilized and dispersed is collected. The remaining solid phase is high-purity zinc oxide, and the content of zinc element in the high-purity zinc oxide is 75%-79% (that is, the purity of zinc oxide can reach 93.5%-98.5%);

[0046] The XRD analysis results of secondary zinc-containing dust are as follows: Figure 2 As shown, from Figure 2 It can be seen that the main phases in the secondary zinc-containing dust are PbCl2, ZnO, CdCl2, KPb2Cl5, K2ZnCl5, NaCl, KCl, and SnCl2;

[0047] Step 3, adding the secondary zinc-containing dust into excess dilute hydrochloric acid and mixing to make pulp, the purpose of adding excess dilute hydrochloric acid is to fully dissolve zinc oxide to obtain zinc chloride, during the dissolution, the temperature is controlled at 50-70° C. by a water bath method, while adding dilute hydrochloric acid and stirring, and measuring the pH index at any time until the pH is 1-3; after full dissolution, precipitation and filtration, a primary zinc-containing filtrate and a primary impurity precipitate are obtained;

[0048] The XRD analysis results of the primary impurity precipitation are shown in Figure 3 ,from Figure 3 It can be seen that the primary impurity precipitation is mainly in the form of PbCl2 and KPb2Cl5;

[0049] The contents of zinc and lead in zinc-containing materials in crude zinc oxide powder, high-purity zinc oxide, secondary zinc-containing dust, primary zinc-containing filtrate and primary impurity precipitate are shown in Table 3:

[0050] Table 3. Content of zinc and lead in different materials (wt%)

[0051]

[0052] Step 4: adding elemental zinc (preferably zinc powder) to the primary zinc-containing filtrate, specifically: determining the content of impurity metal ions in the primary zinc-containing filtrate, and then adding zinc powder (measured by amount of substance) with 2-3 times the content of impurity metal ions;

[0053] Elemental zinc will react with Pb in the primary zinc filtrate 2+ , Cu2+ 、Cd 2+ Cr 3+ Sn 2+ The added elemental zinc will become Zn 2+ The ions dissolve in the solution, and the theory of the replacement reaction is based on the reduction potential and standard Gibbs free energy of each metal element;

[0054] Table 2 and Table 3 show the standard reduction potential and standard Gibbs free energy of each metal, respectively.

[0055] Table 2. Standard reduction potential of various metals

[0056]

[0057]

[0058] Table 3. Standard Gibbs free energy of reduction of each metal (at 25°C)

[0059] <![CDATA[Cr 3+ (aq)+Zn(s)]]> → <![CDATA[Zn 2+ (aq)+Cr(s)]]> -1.00(Kcal / mol) <![CDATA[Fe 2+ (aq)+Zn(s)]]> → <![CDATA[Zn 2+ (aq)+Fe(s)]]> -13.7 (Kcal / mol) <![CDATA[Cd 2+ (aq)+Zn(s)]]> → <![CDATA[Zn 2+ (aq)+Cd(s)]]> -15.2(Kcal / mol) <![CDATA[Pb 2+ (aq)+Zn(s)]]> → <![CDATA[Zn 2+ (aq)+Pb(s)]]> -26.9 (Kcal / mol) <![CDATA[Cu 2+ (aq)+Zn(s)]]> → <![CDATA[Zn 2+ (ac)+Cu(s)]]> -46.4 (Kcal / mol)

[0060] After dissolution, precipitation and filtration, a secondary zinc-containing filtrate and a secondary impurity precipitate are obtained; the secondary zinc-containing filtrate mainly contains Zn 2+ Ions and Cl - ions, and secondary impurity precipitation contains elemental Pb, Cr, Cu, Cd, and Sn, which can be sold directly after collection;

[0061] Step 5, determining the zinc ion content in the secondary zinc-containing filtrate, adding sodium carbonate powder with a zinc ion content of 1.2 times (by amount of substance) to the secondary zinc-containing filtrate, dissolving, precipitating, and filtering to obtain a tertiary impurity filtrate and a tertiary zinc-containing precipitate;

[0062] In this process, the temperature of dissolution and precipitation process was set and controlled to be room temperature, 50℃ and 70℃ respectively. XRD phase analysis was performed on three zinc-containing precipitations at different temperatures. The results are as follows: Figure 4 As shown, from Figure 4 It can be seen that the zinc-containing components in the three zinc-containing precipitations are ZnCO3, Zn4CO3(OH)6H2O, and NaZnH3, and the corresponding reaction equations are:

[0063] ZnCl2(aq)+Na2CO3(aq)=ZnCO3(s)+2NaCl(aq)

[0064] 4ZnCl2(aq)+7Na2CO3(aq)+7H2O=Zn4CO3(OH)6H2O(s)+8NaCl(aq)+6NaHCO3(s)

[0065] 2ZnCl2(aq)+2Na2CO3(aq)+3H2O=2ZnCO3(s)+4NaCl(aq)+2NaZnH3(s).

[0066] As the temperature increases, the amount of NaZnH3 generated decreases.

[0067] High-purity zinc oxide and three zinc-containing precipitates are collected to obtain zinc-rich refined dust.

[0068] The zinc oxide powder can also be obtained by washing with water and heating at 350°C for 1-2 hours.

[0069] The primary impurity precipitate contains lead chloride. The primary impurity precipitate can be further dissolved in hot water at 70-85°C, and then sodium carbonate is added to react to obtain a lead-containing precipitate and a salt solution. The salt solution is dried and the lead-containing precipitate is subjected to XRD phase analysis. The results are as follows: Figure 5 As shown, Figure 5 It is shown that its main components are NaPb2(CO3)2OH and sodium chloride.

[0070] Finally, the NaPb2(CO3)2OH precipitate is filtered out and washed, and finally heated to 350°C and dried to obtain the lead oxide product.

[0071] Beneficial effects: The method of the present invention can be used to perform low-energy resource processing on crude zinc oxide separated by pyrometallurgy, remove impurities in the crude zinc oxide, improve the purity of zinc element, and realize the recycling of valuable metal elements in the crude zinc oxide. The process flow is easy to operate and there are no secondary pollutants.

[0072] Finally, it should be noted that the above description is only a preferred embodiment of the present invention. Under the guidance of the present invention, ordinary technicians in this field can make various similar expressions without violating the purpose and claims of the present invention, and such changes all fall within the scope of protection of the present invention.

Claims

1. A refining method for resource-processing zinc-containing materials by combining pyrometallurgy and hydrometallurgy. Features Follow these steps: Step 1, adding carbon, limestone, silica and bentonite to the zinc-containing material, mixing and then reducing and roasting under high temperature conditions, collecting the zinc element reduced to gaseous state and volatilized, and the zinc element is oxidized in the air after volatilization to obtain crude zinc oxide powder; Step 2: oxidatively roasting the crude zinc oxide powder at high temperature, collecting the volatilized secondary zinc-containing dust, and the remaining solid phase is high-purity zinc oxide; Step 3, adding the secondary zinc-containing dust into excess dilute hydrochloric acid, mixing and slurrying, dissolving, precipitating and filtering to obtain a primary zinc-containing filtrate and a primary impurity precipitate; Step 4: adding elemental zinc to the primary zinc-containing filtrate to carry out a replacement reaction, dissolving, precipitating, and filtering to obtain a secondary zinc-containing filtrate and a secondary impurity precipitate; Step 5, adding excess sodium carbonate to the secondary zinc-containing filtrate, dissolving, precipitating and filtering to obtain a tertiary impurity filtrate and a tertiary zinc-containing precipitate; High-purity zinc oxide and three zinc-containing precipitates are collected to obtain zinc-rich refined dust.

2. The refining method for treating zinc-containing materials by combining pyrometallurgy and hydrometallurgy according to claim 1, Features: In the step 1, reduction roasting is carried out at a temperature of 1100-1350° C. for 15-80 minutes.

3. The refining method for treating zinc-containing materials by combining pyrometallurgy and hydrometallurgy according to claim 1 or 2, Features: In the step 1, blast furnace ash and electric furnace ash are mixed to obtain a zinc-containing material, wherein the zinc-containing material has a zinc content of 10-20% by mass and an iron content of 25-40% by mass; In the mixture of zinc-containing material, carbon, limestone, silica and bentonite, the mass percentage of carbon is 15-35%, the mass percentage of limestone is 2-8%, the mass percentage of silica is ≤5%, and the mass percentage of bentonite is ≤2%.

4. The refining method for treating zinc-containing materials by combining pyrometallurgy and hydrometallurgy according to claim 1, Features: In the step 2, the crude zinc oxide powder is oxygen-roasted at 800-1150° C. for 15-80 minutes, during which the volatilized and dispersed secondary zinc-containing dust is collected.

5. The refining method for resource-processing zinc-containing materials by combining pyrometallurgy and hydrometallurgy according to claim 1, 2 or 4, Features: In the step three, an excess amount of dilute hydrochloric acid is added to the secondary zinc-containing dust for stirring and dissolution, and the temperature is controlled at 50-70° C. until the pH is 1-3, and the zinc oxide in the secondary zinc-containing dust is dissolved into zinc chloride in the primary zinc-containing filtrate.

6. The refining method for resource-processing zinc-containing materials by combining pyrometallurgy and hydrometallurgy according to claim 1, 2 or 4, Features: In the step 5, the three zinc-containing precipitates are washed with water and heated at above 350° C. for 1-2 hours to obtain zinc oxide.

7. The refining method for treating zinc-containing materials by combining pyrometallurgy and hydrometallurgy according to claim 1, 2 or 4, Features: The method further comprises step 6 of dissolving the primary impurity precipitate in hot water at 70-85°C, and then adding sodium carbonate to obtain NaPb 2 (CO 3 ) 2 OH precipitation and sodium chloride solution; NaPb 2 (CO 3 ) 2 The OH precipitate is filtered out and washed, and finally heated to above 350°C and dried to obtain lead oxide.