Cobalt-chromium-molybdenum alloy bar and preparation method thereof
Through vacuum electromagnetic levitation smelting and forging processes, impurity pollution and environmental problems of cobalt-chromium-molybdenum alloy materials are solved, mechanical strength is improved, high strength requirements of spinal connecting rods are met, and processing costs are reduced.
Patent Information
- Application Number
- CN202411270681.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-11
- Publication Date
- 2024-12-06
AI Technical Summary
The existing cobalt-chromium molybdenum alloy materials have insufficient production capacity, and the electroslag remelting technology has problems such as impurity pollution, environmental pollution and high energy consumption, which affects the mechanical properties and processing costs of the alloy.
The vacuum electromagnetic levitation smelting technology is used to prepare cobalt-chromium-molybdenum alloy rods, avoid impurity pollution through vacuum environment and inert gas protection, and improve the mechanical strength and toughness of the alloy through forging and rolling processes.
The mechanical strength of the cobalt-chromium-molybdenum alloy rod is significantly improved by about 21%, and the impurity content is reduced, meeting the high strength requirements of spinal connecting rods, while reducing environmental pollution and energy consumption.
Smart Images

Figure CN119082554A_ABST
Abstract
Description
Technical Field
[0001] The present invention relates to the technical field of cobalt-chromium-molybdenum alloy preparation, and in particular to a cobalt-chromium-molybdenum alloy rod and a preparation method thereof. Background Art
[0002] The spinal connecting rod product made of TC4 titanium alloy magnetic therapy is a key product for posterior screw-rod surgery of the cervical and thoracic lumbar spine. In addition, most spinal orthopedic surgeries require the orthopedic and corrective functions of the screw-rod system, so the mechanical strength of the material is required to be relatively high. Due to the limitations of production equipment, domestic titanium alloy rods are unstable between batches. After the connecting rod surgery, in the fatigue environment of long-term micro-motion, the screw-rod system plays an important supporting role in correcting the distance and height between vertebrae. The size of the screw seat is directly related to the diameter of the connecting rod to be used. The thinner the connecting rod, the smaller the screw seat, forming a low-profile pedicle screw product. Compared with conventional pedicle screws, it has less stimulation to the surrounding soft tissue and the soft tissue heals faster.
[0003] Cobalt-chromium-molybdenum alloy materials have been used clinically for many years, with controllable safety and much higher mechanical strength than forged titanium alloy bars. At present, there is basically no mass production capacity of cobalt-chromium-molybdenum alloy materials in China, and it mainly relies on imports, resulting in a long production period and high price for cobalt-chromium-molybdenum alloy bars. Therefore, the development of cobalt-chromium-molybdenum alloy bars is imminent.
[0004] The Chinese invention patent with application number CN202110652006.7 discloses a high-cobalt and high-molybdenum superhard high-speed steel and a method for improving its hot working performance. The method comprises the following steps: reacting and smelting industrial pure iron, chromium-containing raw materials, molybdenum-containing raw materials, metal tungsten, metal cobalt, graphite, industrial silicon, manganese-containing raw materials, and vanadium-containing raw materials to obtain molten steel; subjecting the ingot obtained by casting the molten steel to pressurized electroslag remelting to obtain an electroslag ingot; the solidification pressure during the pressurized electroslag remelting process is 1 to 2 MPa; subjecting the electroslag ingot to high-temperature heat treatment and forging in turn to obtain high-cobalt and high-molybdenum superhard high-speed steel forgings.
[0005] The Chinese invention patent with application number CN202110652303.1 discloses a method for comprehensively improving the cast structure of high-speed steel and its magnesium and rare earth microalloying and increasing the solidification pressure. The method comprises the following steps: smelting industrial pure iron, chromium-containing raw materials, molybdenum-containing raw materials, metal tungsten, metal cobalt, graphite, industrial silicon, manganese-containing raw materials, and vanadium-containing raw materials to obtain molten steel; adding magnesium alloy and rare earth to the molten steel under a pressure of 1 to 2 MPa for microalloying to obtain microalloyed molten steel; casting the microalloyed molten steel to obtain an ingot; pressurizing the ingot with electroslag remelting to obtain a high-speed steel electroslag ingot; the solidification pressure during the pressurized electroslag remelting process is 1 to 2 MPa.
[0006] Although the above invention patents all disclose methods for preparing cobalt-chromium-molybdenum alloy materials, the smelting and refining means adopted in the patents are mainly electroslag remelting technology. However, the electroslag remelting technology has the following defects, such as: the slag produced by electroslag remelting contains a certain amount of impurities, such as oxides, silicon, phosphorus, sulfur and other elements. Those skilled in the art know that impurity elements have irreversible and fatal harm to the alloy. For example, too many impurity elements will first cause the alloy to fail to meet the requirements of EU and US standards. Secondly, too many impurity elements will directly affect the mechanical properties of the alloy and the comprehensive properties of the material, such as affecting the stability of the molten pool and reducing the quality and reliability of the material; the exhaust gas discharged during the electroslag smelting process will have a serious impact on the ecological environment, including air pollution, soil pollution and water pollution, especially pollutants such as nitrogen oxides, sulfur dioxide and particulate matter will seriously affect the air quality and increase the processing cost; in addition, electroslag remelting requires a large amount of electricity, and the use of electroslag remelting will greatly increase the processing cost of cobalt-chromium-molybdenum materials; in the process of electroslag remelting, the gas released by the material during the melting process cannot be discharged in a timely and efficient manner, increasing the uncertainty of the material's pores. Summary of the invention
[0007] In view of this, the present invention provides a cobalt-chromium-molybdenum alloy rod and a preparation method thereof. Compared with TC4 titanium alloy rod, the mechanical strength of the cobalt-chromium-molybdenum alloy rod provided by the present invention is increased by about 21%, and the toughness is better than that of TC4 titanium alloy rod, which can meet the strength requirements of special parts such as spinal connecting rods. In addition, the present invention adopts a vacuum electromagnetic suspension melting method, which can not only avoid the generation of pollutants such as nitrogen oxides, but also the present invention adopts a vacuum electromagnetic suspension melting technology so that the alloy material does not contact the crucible during the melting process, thereby effectively controlling the contamination of the alloy by impurity elements.
[0008] In order to achieve the above object, the present invention adopts the following technical solutions:
[0009] The invention provides a cobalt-chromium-molybdenum alloy rod. The cobalt-chromium-molybdenum alloy rod comprises the following components in mass percentage: 26.0-30.0% of chromium (Cr), 5.0-7.0% of molybdenum (Mo), and the balance of cobalt (Co).
[0010] Furthermore, the cobalt is added in the form of sponge cobalt.
[0011] Furthermore, the molybdenum and chromium are added in the form of pure metal powder.
[0012] The present invention also provides a method for preparing the cobalt-chromium-molybdenum alloy rod, comprising the following steps:
[0013] S1. Mix the ingredients according to the composition ratio of 26.0-30.0% chromium (Cr), 5.0-7.0% molybdenum (Mo), and the balance of cobalt (Co), mix them evenly, and press them into electrode blocks;
[0014] S2. The electrode block is melted by vacuum electromagnetic suspension melting technology, wherein the power supply power is 300-450KW, the power supply frequency is 10-15KHz, the melting temperature is 3000-3200°C, the melting atmosphere is inert gas protection, and the melting vacuum is 5.0*10 -3 ~6.7*10 -4 Pa, the crucible capacity is 10-50 kg, the crucible cooling water pressure is 2.8-3 Bar, the centrifugal speed is 350-400 r / min, and the ingot is obtained by smelting 2-3 times;
[0015] S3, after polishing the ingot, forging it at a forging temperature of 1150-1350°C for a holding time of 70-90 min, followed by upsetting and stretching, controlling the total deformation to be 70-90%, and obtaining a forged bar blank; the forging process ensures uniform alloy structure and improves strength;
[0016] S4, polishing and grinding the forged bar billet and then rolling it, wherein the rolling temperature is 1000-1200°C and the holding time is 40-70min, the total deformation of the bar billet is 80-95%, and the alloy strength is ensured by the rolling process;
[0017] S5, annealing the rolled bar blank.
[0018] Furthermore, the smelting vacuum degree in step S2 is 2.0*10 -3 ~6.7*10 -4 Pa.
[0019] Furthermore, in step S2, the crucible cooling water pressure is 3 Bar, and the crucible is a water-cooled copper crucible.
[0020] Furthermore, the inert gas in step S2 is argon.
[0021] Furthermore, step S3 is to perform upsetting 2-3 times and stretching 2-3 times.
[0022] Furthermore, the number of rolling passes in step S4 is 12 to 17 times.
[0023] Furthermore, the annealing treatment in step S5 is carried out under the conditions of 800-1000° C. for 50-80 min and air-cooling to room temperature.
[0024] Compared with the prior art, the present invention has the following beneficial effects:
[0025] 1. The present invention abandons the traditional electroslag remelting smelting technology and directly adopts the vacuum electromagnetic suspension smelting method to prepare the cobalt-chromium-molybdenum alloy rod. This smelting method can solve the current situation of uneven smelting of multiple alloy elements, and can also improve the purity of the multi-alloy element ingot, ensure the uniform composition of the ingot, and the composition deviation of the core surface and the upper and lower parts is extremely small. The impurity content in the final product is much lower than the electroslag remelting method.
[0026] 2. Compared with TC4 titanium alloy rods, the mechanical strength of the cobalt-chromium-molybdenum alloy rods of the present invention is increased by about 21%, and the toughness is better than that of TC4 titanium alloy rods. It has high strength and high toughness requirements and meets the support strength requirements of special parts such as spinal connecting rods.
[0027] 3. The tensile strength of the cobalt-chromium-molybdenum alloy rod of the present invention reaches above 1400 MPa, the grain size is greater than or equal to grade 10, and the grain size is less than 11.5 μm. BRIEF DESCRIPTION OF THE DRAWINGS
[0028] Figure 1 3 is a microstructure diagram of the cobalt-chromium-molybdenum alloy rod prepared in Example 1 of the present invention.
[0029] Figure 2 This is a microstructure diagram of the titanium alloy rod of Comparative Example 1 of the present invention.
[0030] Figure 3 3 is a microstructure diagram of the cobalt-chromium-molybdenum alloy rod prepared in Example 2 of the present invention.
[0031] Figure 4 It is the microstructure diagram of the titanium alloy rod of comparative example 2 of the present invention. DETAILED DESCRIPTION
[0032] The invention provides a cobalt-chromium-molybdenum alloy rod. The cobalt-chromium-molybdenum alloy rod comprises the following components in mass percentage: 26.0-30.0% of chromium (Cr), 5.0-7.0% of molybdenum (Mo), and the balance of cobalt (Co).
[0033] In one embodiment of the present invention, the cobalt is added in the form of sponge cobalt, and the molybdenum and chromium are added in the form of pure metal powders.
[0034] The present invention also provides a method for preparing the cobalt-chromium-molybdenum alloy rod, comprising the following steps:
[0035] S1. Mix the ingredients according to the composition ratio of 26.0-30.0% chromium (Cr), 5.0-7.0% molybdenum (Mo), and the balance of cobalt (Co), mix them evenly, and press them into electrode blocks;
[0036] S2. The electrode block is melted by vacuum electromagnetic suspension melting technology, wherein the power supply power is 300-450KW, the power supply frequency is 10-15KHz, the melting temperature is 3000-3200°C, the melting atmosphere is inert gas protection, and the melting vacuum is 5.0*10 -3 ~6.7*10 -4 Pa, crucible capacity is 10-50 kg, crucible cooling water pressure is 2.8-3 Bar, centrifugal speed is 350-400 r.mm -1 , smelt 2 to 3 times to obtain an ingot;
[0037] S3, after polishing the ingot, forging it at a forging temperature of 1150-1350°C for a holding time of 70-90 min, followed by upsetting and stretching, controlling the total deformation to be 70-90%, and obtaining a forged bar blank; the forging process ensures uniform alloy structure and improves strength;
[0038] S4, polishing and grinding the forged bar billet and then rolling it, wherein the rolling temperature is 1000-1200°C and the holding time is 40-70min, the total deformation of the bar billet is 80-95%, and the alloy strength is ensured by the rolling process;
[0039] S5, annealing the rolled bar blank.
[0040] In one embodiment of the present invention, the smelting vacuum degree in step S2 is 2.0*10 -3 ~6.7*10 -4 Pa.
[0041] In one embodiment of the present invention, the crucible cooling water pressure in step S2 is 3 Bar, and the crucible is a water-cooled copper crucible.
[0042] In one embodiment of the present invention, the inert gas in step S2 is argon.
[0043] In one embodiment of the present invention, the main parameters of the vacuum electromagnetic suspension melting technology in step S2 are a crucible capacity of 50 kg, a power supply power of 450 kW, a power supply frequency of 10 kHz, a maximum melting temperature of 3200 ° C, an argon atmosphere, and a limit vacuum of 6.7*10 -4 Pa, the crucible cooling water pressure is 3Bar, the centrifugal speed is 400r.mm-1, and the ingot is obtained by smelting twice.
[0044] In one embodiment of the present invention, step S3 is upsetting 2-3 times and stretching 2-3 times. More preferably, step S3 is upsetting 2 times and stretching 2 times.
[0045] In one embodiment of the present invention, the number of rolling passes in step S4 is 12 to 17 times.
[0046] In one embodiment of the present invention, the annealing treatment condition in step S5 is 800-1000° C. for 50-80 min and air-cooling to room temperature. More preferably, the annealing treatment condition in step S5 is 980° C. for 70 min.
[0047] In order to make the purpose, technical solution and advantages of the present invention clearer, the technical solution of the present invention will be described clearly and completely below. Obviously, the described embodiments are only part of the embodiments of the present invention, not all of the embodiments. Based on the embodiments of the present invention, all other embodiments obtained by ordinary technicians in this field without creative work belong to the scope of protection of the present invention.
[0048] The experimental methods or test methods described in the following examples are conventional methods unless otherwise specified; the raw materials and auxiliary agents are obtained from conventional commercial channels or prepared by conventional methods unless otherwise specified.
[0049] Example 1
[0050] A method for preparing a cobalt-chromium-molybdenum alloy rod, the specific steps are as follows:
[0051] S1. Add 27.0% Cr and 6.0% Mo into sponge cobalt, mix well and press into electrode blocks using a hydraulic press;
[0052] S2. The electrode block is melted by vacuum electromagnetic suspension melting technology. The process parameters of the vacuum electromagnetic suspension melting technology are as follows: crucible capacity is 50 kg, power supply power is 450 KW, power supply frequency is 10 KHz, maximum melting temperature is 3200 ° C, melting atmosphere is argon protection, and ultimate vacuum degree is 6.7*10 -4 Pa, crucible cooling water pressure is 3Bar, centrifugal speed is 400r.mm -1 , smelt twice to obtain an ingot;
[0053] S3, the ingot is polished and then forged, heated to 1300°C and kept warm for 90 minutes, and then subjected to two upsetting and two drawing operations, from a Φ130 billet × Lmm to a Φ55 billet × Lmm, with the total deformation controlled to 78.9%, to obtain a forged bar blank;
[0054] S4, the forged bar billet is polished and ground and then rolled, heated to 1150°C and kept at this temperature for 70 minutes, and then rolled through 14 passes, from Φ55 billet to Φ11.5×Lmm, with a total deformation of 94.7%;
[0055] S5. The rolled bar blank is annealed in an atmospheric furnace at 980°C for 70 minutes, and then air-cooled to room temperature.
[0056] Performance Testing
[0057] 1) The chemical composition of the ingot in step S2 was tested, and the results are shown in Table 1:
[0058] Table 1 Chemical composition of ingot cast in Example 1
[0059] element Cr / % Fe / % Mn / % Mo / % Ni / % Si / % C / % N / % Example - Top 27.06 0.14 <0.01 5.96 0.015 0.038 0.061 0.004 Example - Next 27.02 0.12 <0.01 5.93 0.018 0.035 0.058 0.004 average value 27.04 0.13 <0.01 5.94 0.016 0.036 0.059 0.004
[0060] 2) The mechanical properties of the bar after annealing in step S5 were tested according to the method described in ISO 6892-1:2019. The results are shown in Table 2:
[0061] Table 2 Mechanical properties and grain size of the rod in Example 1
[0062]
[0063]
[0064] The microstructure of the rod in Example 1 is shown in Figure 1 .
[0065] Depend on Figure 1 As shown in Table 2, the cobalt-chromium-molybdenum alloy rod prepared in the embodiment of the present invention has uniform structure and stable mechanical properties. The average grain size is less than 11.2 μm, which reaches the international level.
[0066] Comparative Example 1
[0067] The difference between Comparative Example 1 and Example 1 is that Comparative Example 1 is a TC4 titanium alloy rod, and the TC4 titanium alloy rod is set according to the composition ratio of TC4 in GB / T 3620.1-2016 "Titanium and Titanium Alloy Grades and Chemical Compositions", and the alloy elements in the sponge titanium are Al / %: 6.20, V / %: 4.3, Fe / %: 0.20, O / %: 0.165, and the subsequent smelting, forging, and rolling processes are consistent with Example 1.
[0068] 1) The chemical composition test results of the TC4 titanium alloy ingot are shown in Table 3:
[0069] Table 3 Chemical composition of conventional TC4 titanium alloy ingot
[0070] element Al / % V / % Fe / % C / % N / % O / % H / % Detection value 1 6.24 4.38 0.204 0.009 0.005 0.165 0.0006 Detection value 2 6.19 4.31 0.199 0.010 0.004 0.162 0.0006
[0071] 2) The mechanical properties of TC4 titanium alloy bars were tested according to the method described in ISO 6892-1:2019. The results are shown in Table 4:
[0072] Table 4 Mechanical properties and grain size of rods in comparative example 1
[0073]
[0074] The microstructure of the rod of Comparative Example 1 is shown in Figure 2 .
[0075] From Table 4 and Figure 2 It can be seen that the mechanical properties of the conventional TC4 titanium alloy rod are far lower than those of the cobalt-chromium-molybdenum alloy rod prepared in Example 1.
[0076] Example 2
[0077] The ingot prepared in Example 1 was used to prepare a Φ5.0 mm wire, and the specific steps were as follows:
[0078] 1) The ingot is polished and then forged, heated to 1300° C. and kept warm for 90 min, and then subjected to two upsetting and two drawing operations, from a Φ130 billet×Lmm to a Φ55 billet×Lmm, with the total deformation controlled to be 78.9%, to obtain a forged bar blank;
[0079] 2) The forged bar billet is polished and ground before rolling, heated to 1150°C and kept at this temperature for 70 minutes, and then rolled through 14 passes, from Φ55 billet to Φ11.5×Lmm, with a total deformation of 94.7%;
[0080] 3) Drawing the rolled billet, heating it to 1000°C, and drawing it through 6 passes, from Φ11.5 billet to Φ5.4×Lmm, with a total deformation of 77.9%;
[0081] 4) The drawn rod blank is annealed in an atmospheric furnace at 980° C. for 70 min, and air-cooled to room temperature to obtain a Φ5.0 mm wire.
[0082] The mechanical properties of the wire material described in Example 2 were tested, and the results are shown in Table 5:
[0083] Table 5 Mechanical properties and grain size of the wire material of Example 2
[0084]
[0085] The microstructure of the rod in Example 2 is shown in Figure 3 .
[0086] Comparative Example 2
[0087] The ingot prepared in Comparative Example 1 was used to prepare a Φ5.0 mm wire, and the specific steps were as follows:
[0088] 1) The ingot is polished and then forged, heated to 1150° C. and kept warm for 90 min, and then subjected to two upsetting and two drawing operations, from a Φ130 billet×Lmm to a Φ55 billet×Lmm, with the total deformation amount controlled to 78.9%, to obtain a forged bar blank;
[0089] 2) The forged billet is polished and ground before rolling, heated to 970°C for 70 minutes, and then rolled through 14 passes, from Φ55 billet to Φ11.5×Lmm, with a total deformation of 94.7%;
[0090] 3) Drawing the rolled bar billet, heating it to 920°C, and drawing it through 6 passes, from Φ11.5 billet to Φ5.4×Lmm, with a total deformation of 77.9%;
[0091] 4) The drawn rod blank is annealed in an atmospheric furnace at 720° C. for 70 min, and air-cooled to room temperature to obtain a Φ5.0 mm wire.
[0092] The mechanical properties of the wire material described in Example 2 were tested, and the results are shown in Table 6:
[0093] Table 6 Mechanical properties and grain size of wire material in comparative example 2
[0094]
[0095] The microstructure of the rod of Comparative Example 2 is shown in Figure 4 .
[0096] The wire prepared in Example 2 and the wire prepared in Comparative Example 2 were placed in HF solutions of the same concentration, and corrosion resistance tests were performed for the same period of time. The corrosion resistance of the two was observed with the naked eye. The results showed that the wire prepared in Example 2 was much less corroded than the wire prepared in Comparative Example 2.
[0097] By comparison, it can be seen that the mechanical properties of the wire prepared in Example 2 are far superior to those of Comparative Example 2. Compared with Comparative Example 2, the tensile strength of the wire prepared in Example 2 of the present invention is increased by about 21.84%. The cobalt-chromium-molybdenum alloy wire prepared in Example 2 provides reliable strength requirements and excellent corrosion resistance for spinal connecting rod medical implants.
[0098] The above is only a preferred embodiment of the present invention. It should be pointed out that for ordinary technicians in this technical field, several improvements and modifications can be made without departing from the principle of the present invention. These improvements and modifications should also be regarded as the scope of protection of the present invention.
Claims
1. A cobalt-chromium-molybdenum alloy bar, characterized in that: The cobalt-chromium-molybdenum alloy rod comprises the following components in mass percentage: 26.0-30.0% chromium, 5.0-7.0% molybdenum, and the balance of cobalt.
2. The cobalt-chromium-molybdenum alloy rod according to claim 1, characterized in that: The cobalt was added in the form of sponge cobalt.
3. The cobalt-chromium-molybdenum alloy rod according to claim 1, characterized in that: The molybdenum and chromium are added in the form of pure metal powders.
4. The method for preparing the cobalt-chromium-molybdenum alloy rod according to claim 1, characterized in that: The following steps are involved: S1. The ingredients of the cobalt-chromium-molybdenum alloy rod according to claim 1 are prepared, mixed evenly and pressed into an electrode block; S2. The electrode block is melted by vacuum electromagnetic suspension melting technology, wherein the power supply power is 300-450KW, the power supply frequency is 10-15KHz, the melting temperature is 3000-3200°C, the melting atmosphere is inert gas protection, and the melting vacuum is 5.0*10 -3 ~6.7*10 -4 Pa, the crucible capacity is 10-50 kg, the crucible cooling water pressure is 2.8-3 Bar, the centrifugal speed is 350-400 r / min, and the ingot is obtained by smelting 2-3 times; S3, polishing the ingot and then forging it, the forging temperature is 1150-1350°C, the holding time is 70-90min, followed by upsetting and stretching, controlling the total deformation amount to 70-90%, to obtain a forged bar blank; S4, polishing and grinding the forged bar billet and then rolling it, wherein the rolling temperature is 1000-1200°C and the holding time is 40-70min, and the total deformation of the bar billet is 80-95%; S5, annealing the rolled bar blank.
5. The method for preparing the cobalt-chromium-molybdenum alloy rod according to claim 4, characterized in that: The melting vacuum degree in step S2 is 2.0*10 -3 ~6.7*10 -4 Pa.
6. The method for preparing the cobalt-chromium-molybdenum alloy rod according to claim 4, characterized in that: In step S2, the crucible cooling water pressure is 3 Bar, and the crucible is a water-cooled copper crucible.
7. The method for preparing the cobalt-chromium-molybdenum alloy rod according to claim 4, characterized in that: The inert gas in step S2 is argon.
8. The method for preparing the cobalt-chromium-molybdenum alloy rod according to claim 4, characterized in that: Step S3: upsetting 2-3 times, and stretching 2-3 times.
9. The method for preparing the cobalt-chromium-molybdenum alloy rod according to claim 4, characterized in that: The number of rolling passes in step S4 is 12 to 17.