Iron-based alloy powder and preparation method and application thereof

By preparing iron-based alloy powders with high spherical shape, low oxygen content and good flowability, the problems of high preparation cost and low yield of powder materials in the laser spraying process are solved, and the effect of reducing production costs and increasing yield is achieved.

CN119082597APending Publication Date: 2024-12-06JIANGMEN HONGJIA NEW MATERIAL TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411032645.3
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-30
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The powder material preparation process used in the existing laser spraying process has problems of high manufacturing cost and low yield, and it is difficult to meet the requirements of high spherical shape, good fluidity and low oxygen content of powder materials.

Method used

Using a preparation method of iron-based alloy powder, the components are heated and melted and the residue removal agent and deoxidant are added, and water atomization is carried out to make powder. Combined with cooling, solidification, centrifugal dehydration and drying steps, a high spherical shape is produced. , iron-based alloy powder with low oxygen content and good fluidity.

Benefits of technology

The high pineapple density, low oxygen content and good fluidity of the iron-based alloy powder are achieved, which reduces production costs, increases output, and meets the use requirements of the laser spraying process.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082597A_ABST
    Figure CN119082597A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of powder metallurgy material preparation, and particularly discloses iron-based alloy powder and a preparation method and application thereof. The alloy comprises the following components in percentage by weight: 15.0%-20.0% of Cr, 5.0%-10.0% of Ni, 1.5%-2.5% of Mo, 0.5%-1.0% of Nb, 0.5%-1.0% of Si, 0.8%-1.0% of B, 0.10%-0.15% of C and 65%-75% of Fe. According to the iron-based alloy powder and the preparation method thereof, the types and proportions of all the raw material components are reasonably adjusted, and the prepared iron-based alloy powder is approximately spherical, has the performance of high apparent density, low oxygen content and good fluidity, is low in manufacturing cost and high in productivity and can meet the use requirements of the laser spraying process.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of powder metallurgy material preparation, and in particular to an iron-based alloy powder and a preparation method and application thereof. Background Art

[0002] Laser spraying is a method of injecting powder into a laser beam with an appropriate powder feeding tube, melting the powder with the laser beam, and spraying it onto the substrate surface by powder feeding gas and gravity to form a coating. Since the alloy preparation process is characterized by non-equilibrium metallurgy, the alloy strengthening layer prepared by it often has the characteristics of special organizational structure and metallurgical combination of strengthening layer interface. The strengthening layer of various mechanical parts after repair shows high wear resistance, corrosion resistance, fatigue resistance, oxidation resistance and other high performance. As an advanced green manufacturing process, laser spraying technology is widely used in surface remanufacturing projects of key parts in mining machinery, metallurgical machinery, engineering machinery and other fields.

[0003] With the maturity and popularization of laser spraying technology, the application fields of laser spraying process are also increasing. The application in different fields puts forward more requirements on the powder materials used in laser spraying process: such as high purity of powder materials; low oxygen content to ensure the formation of spray layers without pores and slag inclusions; powder materials have good fluidity and high bulk ratio, and can enter the molten pool evenly and uninterruptedly, requiring the powder materials to be spherical or nearly spherical.

[0004] At present, the main process for preparing powder materials used in laser spraying is gas atomization, but it has the disadvantages of high manufacturing cost and low output, which seriously limits its application.

[0005] Therefore, it is necessary to provide an iron-based alloy powder and a preparation method and application thereof to ensure that the powder has the advantages of high sphericity, good fluidity and low oxygen content, while reducing production costs and increasing output. Summary of the invention

[0006] The present invention aims to solve at least one of the technical problems existing in the above-mentioned prior art. To this end, the present invention provides an iron-based alloy powder and a preparation method and application thereof, which ensures that the powder has the advantages of high sphericity, good fluidity and low oxygen content, while reducing production costs and increasing output.

[0007] A first aspect of the present invention provides an iron-based alloy powder.

[0008] Specifically, an iron-based alloy powder includes the following components in weight percentage: Cr 15.0-20.0%, Ni 5.0-10.0%, Mo 1.5-2.5%, Nb 0.5-1.0%, Si 0.5-1.0%, B 0.8-1.0%, C 0.10-0.15%, and the balance is Fe.

[0009] Preferably, an iron-based alloy powder comprises the following components, in weight percentage: Cr 15.0-18.5%, Ni 5.0-10.0%, Mo 1.5-2.5%, Nb 0.5-1.0%, Si 0.5-1.0%, B 0.8-1.0%, C 0.10-0.15%, Fe 68-75%.

[0010] Preferably, the iron-based alloy powder further comprises inevitable impurities; the content of the inevitable impurities does not exceed 0.305%.

[0011] Preferably, the unavoidable impurities include Mn, P, and S.

[0012] Further preferably, Mn<0.30%, P<0.003%, S<0.003%; wherein S+P<0.005%.

[0013] Cr (chromium): Cr is the main alloying element. When the content exceeds 12%, the spraying material has good high-temperature oxidation resistance and oxidation corrosion resistance. At the same time, it can increase the hardenability of the spraying material and form chromium-containing carbides with C, thereby improving the wear resistance of the material.

[0014] Ni (nickel): Ni has a lattice constant similar to that of γ-iron and can form a continuous solid solution, which is beneficial to improving the hardenability of steel; Ni can reduce the critical point and increase the stability of austenite, so its quenching temperature can be reduced and the hardenability is good. Therefore, nickel can improve the strength, toughness, hardenability and corrosion resistance of coating materials.

[0015] Mo (Molybdenum): Mo can reduce the tendency of carbides to form a continuous network on the grain boundary and increase the wear resistance of the surface layer. In addition, Mo element also has the effect of refining grains, which can improve the toughness of the material and reduce brittleness.

[0016] Nb (Niobium): Nb is a carbide-forming element that can significantly improve the hardness and wear resistance of the material. At the same time, the Nb element also has the effect of refining the grains, which can improve the toughness of the material and reduce its brittleness.

[0017] Si (Silicon): The Si element can not only increase the hardness of the coating, but also lower the melting point of the alloy and improve wettability; in addition, as a deoxidizer in the smelting process, it can reduce the oxygen content in the powder.

[0018] B (boron): trace B element can not only improve the hardness of the coating, but also significantly promote the surface tension of the alloy liquid, which is conducive to the formation of spherical powder. In addition, B is a low melting point, easily oxidized element, which is more easily oxidized than Cr, Ni, etc. In the atomization process, B preferentially reacts with O 2 The reaction generates B oxides, which are adsorbed and removed by the slag-forming agent during the atomization process, thereby reducing the oxygen content in the powder.

[0019] C (carbon): The C element forms metal carbide (MeC) with other alloy elements in the alloy powder material. The content and distribution of metal carbides can significantly increase the wear resistance of the material and achieve the effect of secondary hardening. The C content has a great influence on the strength, plasticity, toughness, wear resistance and welding performance of the spray coating.

[0020] A second aspect of the present invention provides a method for preparing an iron-based alloy powder.

[0021] Specifically, the following steps are included:

[0022] (1) heating and smelting the components, adding a slag remover and a deoxidizer, standing the slag to obtain an iron-based alloy melt;

[0023] (2) pouring the iron-based alloy melt obtained in step (1), atomizing the mixture with water, cooling and solidifying the mixture to obtain a cooled powder;

[0024] (3) centrifugally dehydrating the cooled powder obtained in step (2) to obtain a semi-finished wet powder, and drying the semi-finished wet powder to obtain an iron-based alloy powder;

[0025] In step (2), the pouring temperature is 1630-1660°C;

[0026] In step (2), the water temperature of the water atomization is 30-50°C.

[0027] Preferably, the pouring temperature is 1630-1660°C.

[0028] Further preferably, the pouring temperature is 1640-1645°C.

[0029] Preferably, the water temperature of the water atomization is 40-45°C.

[0030] Preferably, in step (1), the heating and smelting temperature is 1650-1670°C.

[0031] Further preferably, in step (1), the heating and smelting temperature is 1655-1660°C.

[0032] Preferably, in step (1), the deoxidizer comprises metallic silicon particles.

[0033] Preferably, in step (1), the amount of the deoxidizer added is 0.50-0.70% of the total mass of the components.

[0034] Preferably, in step (1), the deslagging agent includes brand F2 deslagging agent.

[0035] Preferably, in step (1), the standing time is 1 to 3 minutes.

[0036] Further preferably, in step (1), the standing time is 3 minutes.

[0037] Preferably, in step (2), the pressure of the water atomization powder making is 8 to 14 MPa.

[0038] Further preferably, in step (2), the pressure of the water atomization powder making is 9 to 11 MPa.

[0039] Preferably, the water atomization spray plate for water atomization powder making contains 4 nozzles.

[0040] Preferably, in step (2), the iron-based alloy melt obtained in step (1) is poured into an atomizing tundish.

[0041] More preferably, the temperature inside the atomizing tundish is 1100-1300°C.

[0042] Preferably, in step (2), the water atomization powder making step further comprises the iron-based alloy melt flowing out from the guide tube of the atomization tundish, and the flowing iron-based alloy melt is crushed by high-pressure water to obtain alloy powder droplets.

[0043] Further preferably, the guide tube is made of corundum or zirconium oxide.

[0044] Further preferably, the diameter of the flow guide tube is 5.5-8.5 mm.

[0045] Preferably, in step (3), the moisture content of the semi-finished wet powder is 3-8%.

[0046] Further preferably, in step (3), the moisture content of the semi-finished wet powder is 5.5-6.5%.

[0047] Preferably, in step (3), the drying temperature is 120-180° C., the drying time is 6-12 h, and the drying speed is 7-12 rpm.

[0048] Further preferably, in step (3), the drying temperature is 160-175° C., the drying time is 8-10 h, and the drying speed is 8-10 rpm.

[0049] A third aspect of the present invention provides an application of an iron-based alloy powder in the field of laser spraying.

[0050] Compared with the prior art, the beneficial effects of the present invention are as follows:

[0051] The invention reasonably adjusts the types and proportions of various raw material components to obtain an iron-based alloy powder that is nearly spherical and has the properties of high bulk density, low oxygen content and good fluidity. At the same time, the manufacturing cost is low and the production capacity is high, which can meet the use requirements of the laser spraying process. BRIEF DESCRIPTION OF THE DRAWINGS

[0052] Figure 1 This is a microscopic morphology analysis diagram of the iron-based alloy powder of Example 1 under a scanning electron microscope;

[0053] Figure 2 This is a microscopic morphology analysis diagram of the iron-based alloy powder of Example 2 under a scanning electron microscope;

[0054] Figure 3 This is a microscopic morphology analysis diagram of the iron-based alloy powder of Example 3 under a scanning electron microscope;

[0055] Figure 4 This is a microscopic morphology analysis diagram of the iron-based alloy powder of Comparative Example 1 under a scanning electron microscope;

[0056] Figure 5 This is a microscopic morphology analysis diagram of the iron-based alloy powder of Comparative Example 2 under a scanning electron microscope. DETAILED DESCRIPTION

[0057] In order to make the technical scheme of the present invention more clearly understood by those skilled in the art, the following embodiments are listed for illustration. It should be pointed out that the following embodiments do not limit the protection scope of the present invention.

[0058] Unless otherwise specified, the raw materials, reagents or devices used in the following examples can be obtained from conventional commercial sources or by existing known methods.

[0059] Example 1

[0060] An iron-based alloy powder and a preparation method thereof.

[0061] The iron-based alloy powder includes the following components by weight percentage: 17.5% Cr, 6.5% Ni, 2.0% Mo, 0.65% Nb, 0.65% Si, 0.95% B, 0.12% C, and the balance is Fe.

[0062] The impurity contents satisfy Mn<0.30wt%, P<0.0025wt%, S<0.002wt%.

[0063] The specific preparation method is as follows:

[0064] (1) The components were heated and smelted at 1660° C., and slag remover and metallic silicon particles were added. The amount of metallic silicon particles added was 0.65% of the total mass of the components. After standing for 3 minutes, the slag was removed to obtain an iron-based alloy melt.

[0065] (2) The iron-based alloy melt obtained in step (1) is poured into an atomizing tundish at a pouring temperature of 1640° C. The temperature inside the atomizing tundish is 1150° C. Then, the iron-based alloy melt flows out from a guide tube of the atomizing tundish. The guide tube is made of corundum and has a diameter of 6.5 mm. The flowing iron-based alloy melt is crushed by high-pressure water. The pressure of the high-pressure water (the pressure of water atomization powder making) is 10 MPa, and the temperature of the high-pressure water (the water temperature of water atomization) is 40° C. The water atomization spray plate has 4 nozzles to obtain alloy powder droplets. After cooling and solidification, a cooled powder is obtained.

[0066] (3) The powder obtained in step (2) is centrifugally dehydrated after cooling to obtain a semi-finished wet powder with a moisture content of 5.5%, and the semi-finished wet powder is vacuum dried at a temperature of 160° C., a time of 10 h, and a rotation speed of 10 rpm. The powder is further subjected to ultrasonic vibration screening using an 80 / 270 mesh screen, and air flow classification to obtain an iron-based alloy powder.

[0067] Example 2

[0068] An iron-based alloy powder and a preparation method thereof.

[0069] The iron-based alloy powder includes the following components by weight percentage: 18.0% Cr, 7.5% Ni, 2.0% Mo, 0.70% Nb, 0.70% Si, 0.90% B, 0.13% C, and the balance is Fe.

[0070] The impurity contents satisfy Mn<0.30wt%, P<0.0025wt%, S<0.002wt%.

[0071] The specific preparation method is as follows:

[0072] (1) The components were heated and smelted at 1655° C., and slag remover and metallic silicon particles were added. The amount of metallic silicon particles added was 0.65% of the total mass of the components. After standing for 3 minutes, the slag was removed to obtain an iron-based alloy melt.

[0073] (2) The iron-based alloy melt obtained in step (1) is poured into an atomizing tundish at a pouring temperature of 1645° C. The temperature inside the atomizing tundish is 1150° C. Then, the iron-based alloy melt flows out from a guide tube of the atomizing tundish. The guide tube is made of corundum and has a diameter of 6.5 mm. The flowing iron-based alloy melt is crushed by high-pressure water. The pressure of the high-pressure water (the pressure of water atomization powder making) is 10 MPa, and the temperature of the high-pressure water (the water temperature of water atomization) is 45° C. The water atomization spray plate has 4 nozzles to obtain alloy powder droplets. After cooling and solidification, a cooled powder is obtained.

[0074] (3) The powder obtained in step (2) is centrifugally dehydrated after cooling to obtain a semi-finished wet powder with a moisture content of 6.5%, and the semi-finished wet powder is vacuum dried at a temperature of 160° C., a time of 10 h, and a rotation speed of 10 rpm. The semi-finished wet powder is further ultrasonically vibrated and screened using a 80 / 270 mesh screen, and air flow graded to obtain an iron-based alloy powder.

[0075] Example 3

[0076] An iron-based alloy powder and a preparation method thereof.

[0077] The iron-based alloy powder includes the following components by weight percentage: 18.5% Cr, 7.0% Ni, 2.0% Mo, 0.75% Nb, 0.68% Si, 0.85% B, 0.10% C, and the balance is Fe.

[0078] The impurity contents satisfy Mn<0.30wt%, P<0.0025wt%, S<0.002wt%.

[0079] The specific preparation method is as follows:

[0080] (1) The components were heated and smelted at 1660° C., and slag remover and metallic silicon particles were added. The amount of metallic silicon particles added was 0.65% of the total mass of the components. After standing for 3 minutes, the slag was removed to obtain an iron-based alloy melt.

[0081] (2) The iron-based alloy melt obtained in step (1) is poured into an atomizing tundish at a pouring temperature of 1640° C. The temperature inside the atomizing tundish is 1150° C. Then, the iron-based alloy melt flows out from the guide tube of the atomizing tundish. The guide tube is made of corundum and has a diameter of 6.5 mm. The flowing iron-based alloy melt is crushed by high-pressure water. The pressure of the high-pressure water (the pressure of water atomization powder making) is 10 MPa, and the temperature of the high-pressure water (the water temperature of water atomization) is 45° C. The water atomization spray plate has 4 nozzles to obtain alloy powder droplets. After cooling and solidification, a cooled powder is obtained.

[0082] (3) The powder obtained in step (2) is centrifugally dehydrated after cooling to obtain a semi-finished wet powder with a moisture content of 6.5%, and the semi-finished wet powder is vacuum dried at a temperature of 160° C., a time of 10 h, and a rotation speed of 10 rpm. The semi-finished wet powder is further ultrasonically vibrated and screened using a 80 / 270 mesh screen, and air flow graded to obtain an iron-based alloy powder.

[0083] Comparative Example 1

[0084] An iron-based alloy powder and a preparation method thereof.

[0085] The difference from Example 3 is that the water temperature of the water atomization in step (2) of Comparative Example 1 is 25°C.

[0086] Comparative Example 2

[0087] An iron-based alloy powder and a preparation method thereof.

[0088] The difference from Example 3 is that the pouring temperature in step (2) of Comparative Example 2 is 1600°C.

[0089] 1. The iron-based alloy powders obtained in Examples 1 to 3 and Comparative Examples 1 to 2 were tested for properties: bulk ratio (AD), flow rate (FR), oxygen content ([O]), and Rockwell hardness. The detailed results are shown in Table 1. AD: refer to GB / T 1479.1-2011; [O]: refer to GB / T 14265-2017; FR: refer to GB / T 1482-2010; Rockwell hardness: refer to GB / T230.1-2018.

[0090] Table 1 Performance test results of various iron-based alloy powders

[0091]

[0092] 2. The microscopic morphology of the iron-based alloy powders of Examples 1 to 3 and Comparative Examples 1 to 2 was analyzed using a scanning electron microscope. Figures 1 to 5 .

[0093] As shown in the figure, Examples 1 to 3 are nearly spherical under a scanning electron microscope, while Comparative Examples 1 to 2 are bean-shaped, and most of the iron-based alloy powders in Comparative Examples 1 to 2 are elongated in shape.

[0094] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution obtained by any modification, equivalent replacement, improvement, etc. made by a person skilled in the art based on the concept of the present invention through logical analysis, reasoning or limited experiments on the basis of the prior art shall be within the scope of protection determined by the claims.

Claims

1. An iron-based alloy powder, It is characterized in that Calculated by weight percentage, it includes the following components: Cr 15.0-20.0%, Ni 5.0-10.0%, Mo 1.5-2.5%, Nb 0.5-1.0%, Si 0.5-1.0%, B 0.8-1.0%, C 0.10-0.15%, Fe 65-75%.

2. The iron-based alloy powder according to claim 1, It is characterized in that Calculated in weight percentage, it includes the following components: Cr 15.0-18.5%, Ni 5.0-10.0%, Mo 1.5-2.5%, Nb 0.5-1.0%, Si 0.5-1.0%, B0.8-1.0%, C 0.10-0.15%, and Fe 68-75%.

3. The iron-based alloy powder according to claim 1, It is characterized in that The iron-based alloy powder further includes inevitable impurities; the content of the inevitable impurities does not exceed 0.305%.

4. The iron-based alloy powder according to claim 1, It is characterized in that The unavoidable impurities include Mn, P, and S.

5. A method for preparing the iron-based alloy powder according to any one of claims 1 to 4, It is characterized in that The following steps are involved: (1) heating and smelting the components, adding a slag remover and a deoxidizer, standing the slag to obtain an iron-based alloy melt; (2) pouring the iron-based alloy melt obtained in step (1), atomizing the mixture with water, cooling and solidifying the mixture to obtain a cooled powder; (3) centrifugally dehydrating the powder obtained in step (2) after cooling to obtain a semi-finished wet powder, and drying it to obtain an iron-based alloy powder; In step (2), the pouring temperature is 1630-1660°C; In step (2), the water temperature of the water atomization is 30-50°C.

6. The preparation method according to claim 5, It is characterized in that In step (1), the heating and smelting temperature is 1650-1670°C.

7. The preparation method according to claim 5, It is characterized in that In step (2), the pressure of the water atomization powder making is 8 to 14 MPa.

8. The preparation method according to claim 5, It is characterized in that In step (3), the moisture content of the semi-finished wet powder is 3-8%.

9. The preparation method according to claim 5, It is characterized in that In step (3), the drying temperature is 120-180° C., the drying time is 6-12 h, and the drying speed is 7-12 rpm.

10. Use of the iron-based alloy powder according to any one of claims 1 to 4 in the field of laser spraying.