Steel wire rod for 1960MPa-grade steel strand, preparation method, steel wire and steel strand
By adding V to the steel stranded wire strips and using aerosol cooling technology, production costs were successfully reduced, and the problem of high cost of 1960MPa steel stranded wire strips in the prior art was solved, achieving cost-effectiveness improvement.
Patent Information
- Application Number
- CN202411227971.X
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-03
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-03
AI Technical Summary
The production cost of existing 1960MPa steel strands is relatively high, which leads to difficulties in market development.
By adding a small amount of V to the steel composition and using a cooling method combined with air cooling after rolling, chemical components were developed: C: 0.78% to 0.84%, Si: 0.17% to 0.35%, Mn: 0.50 %~0.90%, Cr: 0.10%~0.20%, V: 0.04%~0.08%, control the spacing between pearlite sheets to be 80nm~100nm, and meet the tensile strength of 1220MPa~1260MPa .
The production cost has been reduced, and the cost of ton of steel has increased by only about 100 yuan, which has improved the market competitiveness of the product.
Smart Images

Figure CN119082607A_ABST
Abstract
Description
Technical Field
[0001] The present application relates to the technical field of steel material preparation, and in particular to a wire rod for 1960MPa grade steel strand and a preparation method, steel wire, and steel strand. Background Art
[0002] In order to improve the safety factor of buildings such as bridges, dams, and mines, there has been a gradual demand for Φ15.24mm 1960MPa steel strands in recent years. Compared with Φ15.24mm 1860MPa steel strands, 1960MPa steel strands can increase the span and strength of buildings while saving steel.
[0003] At present, the basic composition of wire rods for 1960MPa steel strands developed at home and abroad is 82B. Most manufacturers adopt the method of adding 0.08% to 0.12% V on the basis of the national standard 82B composition system. There are also a few southern enterprises that add an appropriate amount of V (about 0.04%) on the basis of 82B and develop it through an offline salt bath method. The method of adding 0.08-0.12% V to 82B increases the cost of steel by about 200 to 300 yuan per ton. The method of adding a small amount of V to 82B and performing salt bath heat treatment at the same time increases the cost by 500 to 600 yuan. Under the current sluggish steel situation, the cost of the designed product is relatively high, which is not conducive to product development and market development. Therefore, how to reduce the production cost of wire rods for 1960MPa steel strands is a technical problem that needs to be solved urgently. Summary of the invention
[0004] The present application provides a 1960MPa grade wire rod for steel strands and a preparation method, steel wire, and steel strands to solve the following technical problems: successfully developing a 1960MPa wire rod for steel strands by continuous casting of small square billets and reducing its production cost.
[0005] In the first aspect, the present application provides a wire rod for a 1960MPa grade steel strand. The chemical composition of the wire rod, measured by mass fraction, includes: C: 0.78% to 0.84%, Si: 0.17% to 0.35%, Mn: 0.50% to 0.90%, Cr: 0.10% to 0.20%, V: 0.04% to 0.08%, P≤0.015%, S≤0.010%, N≤0.0035%, and the remainder is Fe and unavoidable impurities; the metallographic structure of the wire rod is pearlite, and the interlamellar spacing of the pearlite is 80nm to 100nm.
[0006] Optionally, the diameter of the wire rod is 12.5 mm to 13 mm.
[0007] Optionally, the wire rod meets the following properties: tensile strength is 1220MPa-1260MPa, the tensile strength fluctuation value between the head and tail of the wire rod is ≤40MPa, and the tensile strength fluctuation value within the same circle of the wire rod is ≤30MPa.
[0008] In a second aspect, the present application provides a method for preparing the wire rod according to any one embodiment of the first aspect, the method comprising:
[0009] Continuously casting the molten steel with the chemical composition to obtain a cast billet with a set C segregation index and a set porosity and shrinkage level;
[0010] The ingot is heated, rolled and cooled to obtain a wire rod.
[0011] Optionally, the cooling method is a combination of aerosol cooling and air cooling.
[0012] Optionally, the superheat of the molten steel is 10°C to 20°C.
[0013] Optionally, the C segregation index of the ingot is set to ≤1.05, and the porosity and shrinkage level of the ingot is set to ≤1.0.
[0014] In a third aspect, the present application provides a steel wire, the raw material of which is the wire rod described in any one of the embodiments in the first aspect.
[0015] Optionally, the diameter of the steel wire is 5.05 mm to 5.25 mm, and the tensile strength of the steel wire is ≥1960 MPa.
[0016] In a fourth aspect, the present application provides a steel strand, wherein the steel strand comprises the steel wire described in the embodiment of the third aspect.
[0017] The above technical solution provided by the embodiment of the present application has the following advantages compared with the prior art:
[0018] The present application provides a wire rod for a 1960MPa grade steel strand. The chemical composition of the wire rod includes, by mass fraction: C: 0.78% to 0.84%, Si: 0.17% to 0.35%, Mn: 0.50% to 0.90%, Cr: 0.10% to 0.20%, V: 0.04% to 0.08%, P≤0.015%, S≤0.010%, N≤0.0035%, and the remainder is Fe and unavoidable impurities; the metallographic structure of the wire rod is pearlite, and the interlamellar spacing of the pearlite is 80nm to 100nm. This application rationally designs the chemical composition of the wire rod. By adding V, the strength of the original wire rod is controlled within 1220MPa~1260MPa by utilizing the solid solution strengthening of V and the strong cooling of water mist after rolling. By adding Cr, Cr is a medium-strong carbide precipitation element. Adding Cr to high carbon steel can reduce the start and end temperature of the wire rod during the austenite to pearlite phase transformation, and increase the permeability of the steel. Combined with the post-rolling gas mist cooling method, a Φ15.24mm specification 1960Mpa steel strand wire rod was successfully developed. The cost per ton of steel is only increased by about 100 yuan on the basis of 82B, reducing the production cost. BRIEF DESCRIPTION OF THE DRAWINGS
[0019] The accompanying drawings, which are incorporated in and constitute a part of this specification, illustrate embodiments consistent with the present application and, together with the description, serve to explain the principles of the present application.
[0020] In order to more clearly illustrate the embodiments of the present application or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, for ordinary technicians in this field, other drawings can be obtained based on these drawings without paying any creative labor.
[0021] Figure 1 The metallographic structure diagram of the edge of the wire rod provided in the embodiment of the present application;
[0022] Figure 2 A metallographic structure diagram of the core of the wire rod provided in the embodiment of the present application;
[0023] Figure 3 A schematic flow chart of a method for preparing a wire rod provided in an embodiment of the present application. DETAILED DESCRIPTION
[0024] In order to make the purpose, technical solution and advantages of the embodiments of the present application clearer, the technical solution in the embodiments of the present application will be clearly and completely described below in conjunction with the drawings in the embodiments of the present application. Obviously, the described embodiments are part of the embodiments of the present application, not all of the embodiments. Based on the embodiments in the present application, all other embodiments obtained by ordinary technicians in this field without making creative work are within the scope of protection of this application.
[0025] Various embodiments of the present application may be presented in the form of a range; it should be understood that the description in the form of a range is only for convenience and brevity, and should not be understood as a rigid limitation on the scope of the present application; therefore, the range description should be considered to have specifically disclosed all possible sub-ranges and single numerical values within the range. For example, the range description from 1 to 6 should be considered to have specifically disclosed sub-ranges, such as from 1 to 3, from 1 to 4, from 1 to 5, from 2 to 4, from 2 to 6, from 3 to 6, etc., as well as single numbers within the range, such as 1, 2, 3, 4, 5 and 6, which apply regardless of the range. In addition, whenever a numerical range is indicated herein, it is meant to include any cited number (fractional or integer) within the indicated range.
[0026] In addition, in the description of the specification of the present application, the terms "including", "comprising", etc. mean "including but not limited to". In this article, relational terms such as "first" and "second", etc. are only used to distinguish one entity or operation from another entity or operation, and do not necessarily require or imply any such actual relationship or order between these entities or operations. In this article, "and / or" describes the association relationship of associated objects, indicating that three relationships may exist. For example, A and / or B can represent: A exists alone, A and B exist at the same time, and B exists alone. Wherein A and B can be singular or plural. In this article, "at least one" means one or more, and "plurality" means two or more. "At least one", "the following at least one item (items)" or similar expressions refer to any combination of these items, including any combination of single items (items) or plural items (items). For example, "at least one of a, b, or c", or "at least one of a, b, and c", can both mean: a, b, c, ab (i.e., a and b), ac, bc, or abc, where a, b, c can be single or plural, respectively.
[0027] Unless otherwise specified, various raw materials, reagents, instruments and equipment used in this application can be purchased from the market or prepared by existing methods.
[0028] At present, there are usually two methods for developing Φ15.24mm specification 1960MPa steel strand wire rod in China. One is to directly add 0.08-0.12% V on the basis of Φ12.5mm82B; the other method is to strengthen it by adding 0.04-0.08% V at the same time through online or offline salt bath treatment. Both methods lead to high costs, especially the second one. Although the microstructure is better controlled, the cost is 400-500 yuan / ton. This application successfully developed Φ15.24mm specification 1960Mpa steel strand wire rod by adding a small amount of V to the steel composition and combining post-rolling mist cooling with air cooling. The cost per ton of steel increased by about 100 yuan on the basis of 82B, which reduced the production cost and improved the market competitiveness of the product.
[0029] The present application provides a wire rod for a 1960MPa grade steel strand. The chemical composition of the wire rod includes, by mass fraction: C: 0.78% to 0.84%, Si: 0.17% to 0.35%, Mn: 0.50% to 0.90%, Cr: 0.10% to 0.20%, V: 0.04% to 0.08%, P≤0.015%, S≤0.010%, N≤0.0035%, and the remainder is Fe and unavoidable impurities; the metallographic structure of the wire rod is pearlite, and the interlamellar spacing of the pearlite is 80nm to 100nm.
[0030] In the embodiment of the present application, the positive effect of controlling the C content to 0.78% to 0.84% is that carbon is the most important element that determines the mechanical properties of steel. When the carbon content of steel is increased, since cementite is distributed in a network along the pearlite grain boundary, although the hardness continues to increase, the strength begins to decrease, while the plasticity and toughness decrease even lower. Specifically, the C content can be 0.78%, 0.79%, 0.81%, 0.83%, 0.84%, etc.
[0031] The positive effect of controlling the Si content to 0.17% to 0.35% is that the silicon element plays an important role in steelmaking. During steelmaking, the molten steel needs to be deoxidized. The silicon element has a good affinity with oxygen and is easy to produce silicon dioxide to achieve the purpose of deoxidation. Adding silicon to steel can increase the strength and toughness at the same time. Specifically, the Si content can be 0.17%, 0.23%, 0.28%, 0.32%, 0.35%, etc.
[0032] The positive effect of controlling the Mn content to 0.50% to 0.90% is that manganese can increase the strength and hardness of steel, especially in the later drawing process, it can increase the work hardening rate of steel wire. Specifically, the Mn content can be 0.50%, 0.60%, 0.70%, 0.80%, 0.90%, etc.
[0033] The positive effect of controlling the Cr content to 0.10% to 0.20% is that Cr is a medium-strong carbide precipitation element. Adding it to high carbon steel can reduce the start and end temperature of the wire rod during the austenite to pearlite phase transformation, and increase the permeability of the steel. By adding Cr and controlling the cooling with water mist and air cooling on the air cooling line, the difference in the structure between the surface and the core of the wire rod during air cooling of large-sized wire rods can be solved. If the Cr content is too high, it will cause excessive cooling intensity to a certain extent, and it is easy to have an overcooled structure that affects drawing; if the Cr content is too low, it will cause low cooling intensity to a certain extent, and coarse pearlite structure will appear after the wire rod phase transformation. Specifically, the Cr content can be 0.10%, 0.12%, 0.15%, 0.18%, 0.20%, etc.
[0034] The positive effect of controlling the V content to 0.04% to 0.08% is to improve the tensile strength of the wire rod by using the solid solution strengthening of V in high carbon steel. If the V content is too high, the wire rod strength will be too high to a certain extent, resulting in a high wire breakage rate during the drawing process, and the finished stranded wire strength will be too high; if the V content is too low, the wire rod strength will be lower than 1220MPa to a certain extent, and the strength of the steel wire after drawing by the user cannot meet the minimum requirement of 1860MPa. Specifically, the V content can be 0.04%, 0.05%, 0.06%, 0.07%, 0.08%, etc.
[0035] The positive effect of controlling the P content to ≤ 0.015% is that phosphorus in steel will reduce the cold working performance of steel, causing cold brittleness and reducing the plasticity of steel. In particular, the P content should be controlled for deep drawing materials, and should be controlled as low as possible in the present invention. Specifically, the P content can be 0.007%, 0.009%, 0.008%, 0.010%, 0.011%, 0.015%, etc.
[0036] Positive effects of controlling the S content to ≤ 0.010%: S is a harmful element in steel, which reduces the ductility and toughness of steel, damages the corrosion resistance of steel, and has an adverse effect on welding, etc. In this invention, the S content should be controlled as low as possible. Specifically, the S content can be 0.010%, 0.008%, 0.006%, 0.004%, 0.005%, etc.
[0037] The positive effect of controlling the N content to ≤ 0.0035% is that adding N to steel will increase the hardness and strength, but it will also directly lead to a significant decrease in the plasticity and toughness of the steel. As time goes by, the deformation aging will further reduce the plasticity and toughness of the steel, or even significantly reduce it. In severe cases, cracks and tiny pores will appear in low-alloy steel. In this invention, the N content should be controlled as low as possible. Specifically, the N content can be 0.0035%, 0.0030%, 0.0025%, 0.0023%, 0.0020%, 0.0018%, etc.
[0038] The positive effect of controlling the pearlite lamellar spacing to 80nm to 100nm: this kind of organization has higher strength than pearlite with lamellar spacing greater than 100nm, and has better drawing performance than troostite with a spacing less than 80nm. The wire rod designed in this application needs to meet the tensile strength of 1220 to 1260MPa and the drawing performance of directly drawing from Φ12.5 / 13mm to Φ5.05 / 5.25mm. Considering comprehensively, the pearlite lamellar spacing of the wire rod needs to be controlled to 80nm to 100nm. Specifically, the lamellar spacing of the wire rod can be 80nm, 85nm, 90nm, 95nm, 100nm, etc. Figure 1 The metallographic structure diagram of the edge of the wire rod provided in the embodiment of the present application; Figure 2 The core metallographic structure diagram of the wire rod provided in the embodiment of the present application. Figure 1 and Figure 2 , it can be seen that the Φ12.5mm wire rod has better organizational uniformity.
[0039] In an embodiment, the diameter of the wire rod is 12.5 mm to 13 mm.
[0040] The positive effect of controlling the diameter of the wire rod to 12.5mm to 13mm: the drawing process of the wire rod is a work hardening process. The tensile strength of the finished steel wire depends on the tensile strength of the original wire rod superimposed on the work hardening strength during the drawing process. The work hardening strength is directly related to the diameter reduction rate generated during the drawing process. In order to obtain a steel wire strength of more than 1220MPa, the diameter of the original wire rod should be controlled above 12.5mm. Specifically, the diameter of the wire rod can be 12.5mm, 12.6mm, 12.7mm, 12.8mm, 12.9mm, 13mm, etc.
[0041] In an implementation manner, the wire rod needs to meet the following performance requirements: tensile strength is 1220MPa-1260MPa, the tensile strength fluctuation value between the head and tail of the wire rod is ≤40MPa, and the tensile strength fluctuation value of the same circle of the wire rod is ≤30MPa.
[0042] In the above embodiment, the tensile strength of the finished steel wire depends on the drawing work hardening strength and the original strength. When the original wire rod with a specification of 12.5-13 mm is drawn to 5.05-5.25 mm, the strength needs to reach 1960 MPa, and the original wire rod should be controlled above 1220 MPa. The tensile strength of the wire rod can be 1220 MPa, 1255 MPa, 1260 MPa, etc. The fluctuation of the tensile strength of the wire rod head and tail is controlled within 40 MPa, and the tensile strength of the same circle is controlled within 30 MPa. The wire rod shall not be scratched or otherwise damaged in the process of bundling and transportation.
[0043] Figure 3 A schematic flow chart of a method for preparing a wire rod provided in an embodiment of the present application.
[0044] See also Figure 3 The present application provides a method for preparing the wire rod described in any one of the above embodiments, the method comprising:
[0045] S1, continuously casting the molten steel having the chemical composition to obtain a cast billet having a set C segregation index and a set porosity and shrinkage level;
[0046] S2. Heating, rolling and cooling the ingot to obtain wire rod.
[0047] In an embodiment, the cooling method is a combination of aerosol cooling and air cooling.
[0048] In the above embodiment, the pearlite lamellar spacing of the wire rod is controlled to be 80nm to 100nm by combining mist cooling and air cooling on the post-rolling air cooling line, and the tensile strength of the wire rod after rolling off the line is improved by structural strengthening.
[0049] In an embodiment, the superheat degree of the molten steel is 10°C to 20°C.
[0050] In an implementation manner, the C segregation index of the cast billet is set to be ≤1.05, and the porosity and shrinkage levels of the cast billet are set to be ≤1.0.
[0051] Before step S1, the molten iron is smelted in a converter; the molten iron after smelting in the converter is refined to obtain the above-mentioned molten steel, and the positive effect of controlling the process parameters of the above-mentioned continuous casting is to ensure that the wire rod does not break during the drawing process and to ensure the surface quality of the wire rod.
[0052] The product prepared by the wire rod preparation method is the above-mentioned wire rod. The chemical composition and microstructure of the wire rod prepared by the wire rod preparation method can refer to the above-mentioned embodiment. Since the wire rod preparation method adopts part or all of the technical solutions of the wire rod embodiment, it at least has all the beneficial effects brought by the technical solutions of the wire rod embodiment, which will not be described one by one here.
[0053] Based on a general inventive concept, the present application provides a steel wire, the raw material of which is the wire rod described in any one of the above embodiments.
[0054] In an embodiment, the diameter of the steel wire is 5.05 mm to 5.25 mm, and the tensile strength of the steel wire is ≥1960 MPa.
[0055] In the embodiment of the present application, the wire rod is directly drawn without heat treatment to obtain a steel wire with a diameter of 5.05-5.25 mm and a tensile strength of 1960-2060 MPa, which is lower in cost than the current domestic production method. Specifically, the diameter of the steel wire can be 5.05 mm, 5.10 mm, 5.15 mm, 5.20 mm, 5.25 mm, etc., and the tensile strength of the steel wire can be 1960 MPa, 1970 MPa, 1980 MPa, 2000 MPa, 2050 MPa, 2060 MPa, etc.
[0056] Based on a general inventive concept, the present application provides a steel strand, the steel strand comprising the steel wires described in the above embodiments.
[0057] The Φ15.24mm 1960MPa steel strand produced by this method has lower cost.
[0058] The present application will be further described below in conjunction with specific embodiments. It should be understood that these embodiments are intended only to illustrate the present application and are not intended to limit the scope of the present application. The experimental methods for which specific conditions are not specified in the following examples are usually measured according to industry standards. If there is no corresponding industry standard, then the conditions recommended by the manufacturer are followed.
[0059] In the embodiment of the present application, the full process route of the wire rod is obtained:
[0060] Industrial molten iron, scrap steel → 90-ton converter smelting → LF furnace refining → continuous casting of 160mm square billet → billet heating → rough rolling → intermediate rolling → water penetration (primary controlled cooling) → finishing rolling (controlled rolling) → water penetration (secondary controlled cooling) → wire laying → mist cooling + air cooling (tertiary controlled cooling) → coiling → PF line transportation → bundling → packaging and transportation. For more specific chemical composition of wire rod, please refer to Table 1; for preparation process, please refer to Table 2; for the properties of wire rod and steel wire, please refer to Table 3.
[0061] Table 1 Chemical composition of wire rod (wt%)
[0062] Serial number C Si Mn P S N V Cr Example 1 0.81 0.22 0.80 0.014 0.004 0.0026 0.04 0.15 Example 2 0.82 0.23 0.84 0.008 0.005 0.0028 0.05 0.18 Example 3 0.82 0.22 0.85 0.011 0.003 0.0028 0.06 0.17 Example 4 0.84 0.23 0.78 0.012 0.005 0.0032 0.07 0.20 Example 5 0.79 0.17 0.83 0.009 0.006 0.0028 0.06 0.15 Example 6 0.83 0.23 0.81 0.007 0.005 0.0026 0.06 0.18 Comparative Example 1 0.80 0.18 0.80 0.011 0.005 0.0028 -- --
[0063] Table 2 Preparation process parameters of wire rod
[0064] Serial number Superheat℃ Slab C segregation index Porosity and shrinkage level / grade Example 1 20 1.05 0.5 Example 2 18 1.02 0.5 Example 3 20 1.05 1.0 Example 4 18 1.05 0.5 Example 5 19 1.04 1.0 Example 6 20 1.03 0.5 Comparative Example 1 32 1.08 2.5
[0065] Table 3 Properties of wire rod and steel wire
[0066]
[0067] From Tables 1 to 3, it can be seen that the solution of the embodiment of the present application can successfully obtain 1960MPa steel strands and steel wires, meeting the needs of users.
[0068] The above description is only a specific implementation of the present application, so that those skilled in the art can understand or implement the present application. Various modifications to these embodiments will be apparent to those skilled in the art, and the general principles defined herein can be implemented in other embodiments without departing from the spirit or scope of the present application. Therefore, the present application will not be limited to the embodiments shown herein, but will conform to the widest range consistent with the principles and novel features applied for herein.
Claims
1. A 1960MPa grade steel strand wire rod, characterized in that: Measured by mass fraction, the chemical composition of the wire rod includes: C: 0.78% to 0.84%, Si: 0.17% to 0.35%, Mn: 0.50% to 0.90%, Cr: 0.10% to 0.20%, V: 0.04% to 0.08%, P≤0.015%, S≤0.010%, N≤0.0035%, and the remainder is Fe and unavoidable impurities; the metallographic structure of the wire rod is pearlite, and the interlamellar spacing of the pearlite is 80nm to 100nm.
2. The wire rod according to claim 1, characterized in that The diameter of the wire rod is 12.5 mm to 13 mm.
3. The wire rod according to claim 2, characterized in that The wire rod meets the following properties: tensile strength is 1220MPa-1260MPa, the tensile strength fluctuation value between the head and tail of the wire rod is ≤40MPa, and the tensile strength fluctuation value within the same circle of the wire rod is ≤30MPa.
4. A method for preparing a wire rod according to any one of claims 1 to 3, characterized in that: The method comprises: Continuously casting the molten steel with the chemical composition to obtain a cast billet with a set C segregation index and a set porosity and shrinkage level; The ingot is heated, rolled and cooled to obtain a wire rod.
5. The method according to claim 5, characterized in that: The cooling method is a combination of mist cooling and air cooling.
6. The method according to claim 5, characterized in that The superheat degree of the molten steel is 10°C to 20°C.
7. The method according to claim 5, characterized in that The set C segregation index of the ingot is ≤1.05, and the set porosity and shrinkage level of the ingot is ≤1.
0.
8. A steel wire, characterized in that: The raw material of the steel wire is the wire rod according to any one of claims 1 to 3.
9. The steel wire according to claim 8, characterized in that The diameter of the steel wire is 5.05 mm to 5.25 mm, and the tensile strength of the steel wire is ≥1960 MPa.
10. A steel strand, characterized in that: The steel strand comprises the steel wire described in claim 8 or 9.
Citation Information
Patent Citations
Microalloying high strength wire rod
CN101353764A
Production process for 82B wire rod used for high strength prestressed steel wire and wire rod thereof
CN102876983A
Method for reducing hypereutectoid wire rod core network cementite
CN104388826A
Ultrahigh-strength prestressed steel wire rod and production method thereof
CN116179944A
1960-2060 MPa-grade prestressed steel strand and preparation method thereof
CN117845141A
Cited By
A hot-rolled wire rod for 1960MPa grade stranded wire and its manufacturing method
CN120796650B