Steel for hydraulic piston rod and preparation method thereof

By using specific components of steel and nanomaterial combinations in hydraulic piston rods and combining functional coating design, the existing hydraulic piston rod performance problems and environmental protection problems are solved, efficient and environmentally friendly steel preparation is achieved, and the piston rod is improved. Performance and service life.

CN119082608APending Publication Date: 2024-12-06JIANGSU NEW HEYI MASCH CO LTD
View PDF 5 Cites 0 Cited by

Patent Information

Application Number
CN202411233807.X
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-04
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The mechanical and mechanical properties, corrosion resistance, wear resistance and fatigue resistance of existing hydraulic piston rods are insufficient, and the production process is high, low efficiency, and pollute the environment, making it difficult to meet the modern energy-saving and environmental protection requirements.

Method used

Using specific components of steel combined with the combination of nanotitanium nitride and nanochromium carbide, a hydraulic piston rod with excellent mechanical properties, corrosion resistance and fatigue resistance is prepared through vacuum induction furnace smelting, heat treatment and functional coating design. Use steel.

Benefits of technology

It improves the mechanical and mechanical properties, corrosion resistance and fatigue resistance of hydraulic piston rods, extends the service life, simplifies the production process, is suitable for continuous large-scale production, reduces energy consumption and pollution, and meets modern environmental protection requirements.

✦ Generated by Eureka AI based on patent content.
Patent Text Reader

Abstract

The invention discloses steel for a hydraulic piston rod and a preparation method of the steel, and relates to the technical field of metallurgy, the steel comprises a steel body and a functional coating covering the surface of the steel body, and the steel body is prepared from C, Si, Mn, Mo, Co, Nb, Cu, rare earth elements, Zr, Ta, Os, Ga, Ti, B, N, nano titanium nitride, nano chromium carbide, Fe and inevitable impurities; the functional coating is prepared from the following raw materials: a hyperbranched perfluoropolyether urethane acrylate oligomer, (perfluoropropane-2, 2-diyl) bis (4, 1-phenylene) diacrylate, bis (1-vinyl imidazole-2-) ketone, 2-(1-propylene-2-yl) benzo [D] oxazole, an initiator and a solvent, and the functional coating is prepared from the following raw materials: a hyperbranched perfluoropolyether urethane acrylate oligomer, (perfluoropropane-2, 2-diyl) bis (4, 1-phenylene) diacrylate, bis (1-vinyl imidazole-2-) ketone, 2-(1-propylene-2-yl) benzo [D] oxazole, an initiator and a solvent. The steel for the hydraulic piston rod is good in mechanical property, excellent in corrosion resistance, wear resistance and fatigue resistance and long in service life.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metallurgy, and in particular to a steel material for a hydraulic piston rod and a preparation method thereof. Background Art

[0002] With the development of the national engineering machinery industry, the application scope of engineering hydraulic cylinders, as one of the main actuators of hydraulic systems, is becoming wider and wider, and the demand is increasing. As an important component in the hydraulic cylinder, the quality of the piston rod has a huge impact on the normal operation of the entire hydraulic cylinder. The piston rod is a moving part with frequent movements and high technical requirements. It transmits the force acting on the piston and drives the piston to move. The ideal piston rod should have excellent mechanical properties, corrosion resistance, wear resistance and fatigue resistance.

[0003] At present, the existing hydraulic piston rods generally use medium carbon structural steel, such as 45, 40Cr, 42CrMo steel. These bars need to be tempered and heat treated when used as raw materials for machining and cutting. The tempering cost is high and the production efficiency is low. In addition, the tempering process will increase energy consumption and pollute the environment, and there will be some waste loss, which does not meet the current energy-saving and environmental protection requirements. Other types of hydraulic piston rod steel on the market also have more or less technical defects in mechanical properties, corrosion resistance, wear resistance and fatigue resistance, which still need to be further improved.

[0004] In order to solve the above problems, the Chinese invention patent with authorization announcement number CN110669991B discloses a 20MnV6 steel for hydraulic piston rod and a preparation method thereof. The chemical composition and mass percentage of the 20MnV6 steel are: C: 0.17-0.22%, Si: 0.43-0.47%, Mn: 1.47-1.53%, Cr: 0.14-0.16%, V: 0.08-0.20%, Mo≤0.08%, Ni: 0.14-0.16%, Al: 0.030-0.045%, P≤0.010%, S≤0.008%, Cu≤0.10%, N≤0.10%, and the balance is Fe and unavoidable impurities; the preparation method includes converter smelting, LF refining, VD vacuum refining, continuous casting, heating and rolling processes. The invention adopts VN and AlN microalloying composition design, and cooperates with LF, VD, controlled rolling and controlled cooling process to obtain 20MnV6 steel with high strength and high impact toughness. However, the corrosion resistance, fatigue resistance and wear resistance of this material still need to be further improved.

[0005] It can be seen that the development of a hydraulic piston rod steel with good mechanical properties, excellent corrosion resistance, wear resistance and fatigue resistance, and long service life and its preparation method meets market demand, has broad market value and application prospects, and is of great significance to promoting the development of the hydraulic piston rod field. Summary of the invention

[0006] The purpose of the present invention is to overcome the deficiencies of the prior art and to provide a steel material for a hydraulic piston rod having good mechanical properties, excellent corrosion resistance, wear resistance and fatigue resistance, and a long service life, and a preparation method thereof.

[0007] To achieve the above-mentioned purpose, the technical solution adopted by the present invention is: a steel material for a hydraulic piston rod, comprising a steel material body and a functional coating covered on the surface thereof, wherein the steel material body comprises the following components in percentage by mass: C 0.15-0.50wt%, Si 0.12-0.52wt%, Mn 1.0-1.6wt%, Mo 0.05-0.15wt%, Co 0.08-0.12wt%, Nb 0.06-0.10wt%, Cu 0.01-0.06wt%, rare earth elements 0.01-0.05wt%, Zr 0.01-0.06wt%, Ta 0.01-0.03wt%, Os 0.001-0.004wt%, Ga 0.01-0.02wt%, Ti 0.03-0.05wt%, B 0.001-0.003wt%, N 0.003-0.006wt%, nano titanium nitride 0.01-0.03wt%, nano chromium carbide 0.01-0.03wt%, and the rest are Fe and inevitable impurities; the functional coating is made of the following raw materials calculated by weight: 30-50 parts of hyperbranched perfluoropolyether polyurethane acrylate polymer, 1-3 parts of (perfluoropropane-2,2-diyl)bis(4,1-phenylene) diacrylate, 2-4 parts of bis(1-vinyl imidazole-2-)ketone, 1-3 parts of 2-(1-propylene-2-yl)benzo[D]oxazole, 0.8-1.2 parts of initiator, and 30-40 parts of solvent.

[0008] Preferably, the rare earth element is a mixture of Sc, Y, Ce, and Gd in a mass ratio of 1:2:(3-5):1.

[0009] Preferably, the particle size of the nano titanium nitride is 10-80 nm; the particle size of the nano chromium carbide is 20-90 nm.

[0010] Preferably, there is no special requirement for the source of the hyperbranched perfluoropolyether polyurethane acrylate oligomer. In one embodiment of the present invention, the hyperbranched perfluoropolyether polyurethane acrylate oligomer is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN105482686B.

[0011] Preferably, the solvent is at least one of N-methylpyrrolidone and N,N-dimethylformamide; and the initiator is azobisisobutyronitrile.

[0012] Another object of the present invention is to provide a method for preparing the steel for the hydraulic piston rod, comprising the following steps:

[0013] Step S1, smelting raw materials Fe, C-Fe master alloy, Si-Fe master alloy, Mn-Fe master alloy, Mo-Fe master alloy, Co-Fe master alloy, Nb-Fe master alloy, Cu-Fe master alloy, rare earth element-Fe master alloy, Zr-Fe master alloy, Ta-Fe master alloy, Os-Fe master alloy, Ga-Fe master alloy, Ti-Fe master alloy, B-Fe master alloy, and N-Fe master alloy in a vacuum induction furnace, stirring to make the alloy composition uniform, then doping nano-titanium nitride and nano-chromium carbide preheated to 550-650° C. into the smelted alloy melt, and then stirring to make the composition uniform, and the alloy melt after stirring and doping is fully allowed to stand and then cast to obtain an ingot;

[0014] Step S2, sequentially heat treating, polishing, grinding, stamping, and turning the ingot produced in step S1 to obtain a steel body;

[0015] Step S3: After mixing the raw materials of the functional coating evenly, apply them on the surface of the steel body, cure them at 60-70° C. for 1-2 hours, and then dry them at 115-125° C. to constant weight to obtain steel for hydraulic piston rods.

[0016] Preferably, the smelting temperature in step S1 is 1450-1560°C.

[0017] Preferably, the heat treatment in step S2 includes homogenization treatment, normalizing treatment, quenching treatment and tempering treatment performed in sequence.

[0018] Preferably, the temperature of the homogenization treatment is 1160-1270°C, and the holding time is 8-13h; the temperature of the normalizing treatment is 880-930°C, and the holding time is 1-2h, followed by cooling in air; the quenching treatment process is to keep at 860-890°C for 1-3 hours and then water cool; the tempering treatment process is to keep at 250-350°C for 1-3 hours and then cool in air.

[0019] Preferably, the thickness of the functional coating in step S3 is 50-160 μm.

[0020] Due to the application of the above technical solution, the present invention has the following beneficial effects:

[0021] (1) The method for preparing the steel for the hydraulic piston rod disclosed in the present invention has a simple process, convenient operation and control, high preparation efficiency and finished product qualification rate, is suitable for continuous large-scale production, and has a high value for promotion and application.

[0022] (2) The steel for hydraulic piston rod disclosed in the present invention comprises a steel body and a functional coating covered on the surface thereof, wherein the steel body comprises the following components in percentage by mass: C 0.15-0.50wt%, Si 0.12-0.52wt%, Mn 1.0-1.6wt%, Mo 0.05-0.15wt%, Co 0.08-0.12wt%, Nb 0.06-0.10wt%, Cu 0.01-0.06wt%, rare earth elements 0.01-0.05wt%, Zr 0.01-0.06wt%, Ta 0.01-0.03wt%, Os0.001-0.004wt%, Ga 0.01-0.02wt%, Ti 0.03-0.05wt%, B 0.001-0.003wt%, N 0.003-0.006wt%, nano titanium nitride 0.01-0.03wt%, nano chromium carbide 0.01-0.03wt%, the rest is Fe and inevitable impurities; the functional coating is made of the following raw materials calculated by weight: 30-50 parts of hyperbranched perfluoropolyether polyurethane acrylate oligomer, 1-3 parts of (perfluoropropane-2,2-diyl) bis(4,1-phenylene) diacrylate, 2-4 parts of bis(1-vinyl imidazole-2-) ketone, 1-3 parts of 2-(1-propylene-2-yl) benzo[D] oxazole, 0.8-1.2 parts of initiator, and 30-40 parts of solvent. Through the above structural design, the various components and raw materials directly cooperate with each other to make the steel for hydraulic piston rod have good mechanical properties, excellent corrosion resistance, wear resistance and fatigue resistance, and long service life.

[0023] (3) The steel material for hydraulic piston rod disclosed in the present invention, the combination of nano titanium nitride and nano chromium carbide can make the internal structure of the body more compact, play a role of dispersion strengthening, and improve wear resistance and corrosion resistance; the functional coating is made of the following raw materials calculated by weight: 30-50 parts of hyperbranched perfluoropolyether polyurethane acrylate polymer, 1-3 parts of (perfluoropropane-2,2-diyl)bis(4,1-phenylene) diacrylate, 2-4 parts of bis(1-vinylimidazole-2-)ketone, 1-3 parts of 2-(1-propylene-2-yl)benzo[D]oxazole, 0.8-1.2 parts of initiator, and 30-40 parts of solvent. Hyperbranched perfluoropolyether polyurethane acrylate, (perfluoropropane-2,2-diyl)bis(4,1-phenylene), imidazolone and oxazole structures are simultaneously introduced into the molecular structure of the coating. These structures, under the multiple effects of electronic effect, steric effect and conjugation effect, can give the coating excellent corrosion resistance and durability, effectively extend its service life, and provide good protection for the internal steel body; the raw materials containing unsaturated olefinic bonds form an interpenetrating network structure through copolymerization and curing reaction, further improving the above-mentioned properties; and through the reasonable selection of the main body components and the raw material formula for the functional coating preparation, they have good compatibility, are not easy to delaminate, and have good performance stability.

[0024] (4) The steel material for hydraulic piston rod disclosed in the present invention has better mechanical properties, better corrosion resistance, wear resistance and fatigue resistance, and longer service life through reasonable selection of preparation steps, heat treatment processes, etc. and their coordination with each other. DETAILED DESCRIPTION

[0025] The following description is used to disclose the present invention so that those skilled in the art can implement the present invention. The preferred embodiments described below are only examples, and those skilled in the art may think of other obvious variations.

[0026] Example 1

[0027] A steel material for a hydraulic piston rod, comprising a steel material body and a functional coating covered on the surface thereof, wherein the steel material body comprises the following components in percentage by mass: C 0.15wt%, Si 0.12wt%, Mn 1.0wt%, Mo0.05wt%, Co 0.08wt%, Nb 0.06wt%, Cu 0.01wt%, rare earth elements 0.01wt%, Zr 0.01wt%, Ta0.01wt%, Os0.001wt%, Ga 0.01wt%, Ti 0.03wt%, B 0.001wt%, N 0.003wt%, nano titanium nitride 0.01wt%, nano chromium carbide 0.01wt%, and the rest are Fe and inevitable impurities; the functional coating is made of the following raw materials calculated by weight: 30 parts of hyperbranched perfluoropolyether polyurethane acrylate polymer, 1 part of (perfluoropropane-2,2-diyl)bis(4,1-phenylene) diacrylate, 2 parts of bis(1-vinylimidazole-2-)ketone, 1 part of 2-(1-propylene-2-yl)benzo[D]oxazole, 0.8 parts of initiator, and 30 parts of solvent.

[0028] The rare earth element is a mixture of Sc, Y, Ce, and Gd in a mass ratio of 1:2:3:1; the particle size of the nano titanium nitride is 10 nm; the particle size of the nano chromium carbide is 20 nm; the hyperbranched perfluoropolyether polyurethane acrylate polymer is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN105482686B; the solvent is N-methylpyrrolidone; and the initiator is azobisisobutyronitrile.

[0029] A method for preparing the steel material for the hydraulic piston rod comprises the following steps:

[0030] Step S1, smelting the raw materials Fe, C-Fe master alloy, Si-Fe master alloy, Mn-Fe master alloy, Mo-Fe master alloy, Co-Fe master alloy, Nb-Fe master alloy, Cu-Fe master alloy, rare earth element-Fe master alloy, Zr-Fe master alloy, Ta-Fe master alloy, Os-Fe master alloy, Ga-Fe master alloy, Ti-Fe master alloy, B-Fe master alloy, and N-Fe master alloy in a vacuum induction furnace, stirring to make the alloy composition uniform, then doping nano-titanium nitride and nano-chromium carbide preheated to 550° C. into the smelted alloy melt, and then stirring to make the composition uniform, and the alloy melt after stirring and doping is fully allowed to stand and then cast to obtain an ingot;

[0031] Step S2, sequentially heat treating, polishing, grinding, stamping, and turning the ingot produced in step S1 to obtain a steel body;

[0032] Step S3: After mixing the raw materials of the functional coating evenly, apply the mixture on the surface of the steel body, cure at 60° C. for 1 hour, and then dry at 115° C. to constant weight to obtain a steel for a hydraulic piston rod.

[0033] The smelting temperature in step S1 is 1450; the heat treatment in step S2 includes homogenization treatment, normalizing treatment, quenching treatment and tempering treatment performed in sequence; the homogenization temperature is 1160°C, and the holding time is 8h; the normalizing temperature is 880°C, and the holding time is 1h, followed by cooling in air; the quenching process is to keep at 860°C for 1 hour and then water cool; the tempering process is to keep at 250°C for 1 hour and then cool in air.

[0034] The thickness of the functional coating in step S3 is 100 μm.

[0035] Example 2

[0036] A steel material for a hydraulic piston rod, comprising a steel material body and a functional coating covered on the surface thereof, wherein the steel material body comprises the following components in percentage by mass: C 0.25wt%, Si 0.24wt%, Mn 1.2wt%, Mo0.08wt%, Co 0.09wt%, Nb 0.07wt%, Cu 0.02wt%, rare earth elements 0.02wt%, Zr 0.02wt%, Ta0.015wt%, Os0.002wt%, Ga 0.013wt%, Ti 0.035wt%, B 0.0015wt%, N 0.004wt%, nano titanium nitride 0.015wt%, nano chromium carbide 0.015wt%, the rest is Fe and inevitable impurities; the functional coating is made of the following raw materials calculated by weight: 35 parts of hyperbranched perfluoropolyether polyurethane acrylate polymer, 1.5 parts of (perfluoropropane-2,2-diyl)bis(4,1-phenylene) diacrylate, 2.5 parts of bis(1-vinylimidazole-2-)ketone, 1.5 parts of 2-(1-propylene-2-yl)benzo[D]oxazole, 0.9 parts of initiator, and 33 parts of solvent.

[0037] The rare earth element is a mixture of Sc, Y, Ce, and Gd in a mass ratio of 1:2:3.5:1; the particle size of the nano titanium nitride is 30 nm; the particle size of the nano chromium carbide is 40 nm; the hyperbranched perfluoropolyether polyurethane acrylate polymer is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN105482686B; the solvent is N,N-dimethylformamide; and the initiator is azobisisobutyronitrile.

[0038] A method for preparing the steel material for the hydraulic piston rod comprises the following steps:

[0039] Step S1, smelting raw materials Fe, C-Fe master alloy, Si-Fe master alloy, Mn-Fe master alloy, Mo-Fe master alloy, Co-Fe master alloy, Nb-Fe master alloy, Cu-Fe master alloy, rare earth element-Fe master alloy, Zr-Fe master alloy, Ta-Fe master alloy, Os-Fe master alloy, Ga-Fe master alloy, Ti-Fe master alloy, B-Fe master alloy, and N-Fe master alloy in a vacuum induction furnace, stirring to make the alloy composition uniform, then doping nano-titanium nitride and nano-chromium carbide preheated to 580° C. into the smelted alloy melt, and then stirring to make the composition uniform, and the alloy melt after stirring and doping is fully allowed to stand and then cast to obtain an ingot;

[0040] Step S2, sequentially heat treating, polishing, grinding, stamping, and turning the ingot produced in step S1 to obtain a steel body;

[0041] Step S3: After mixing the raw materials of the functional coating evenly, apply the mixture on the surface of the steel body, cure at 63° C. for 1.3 hours, and then dry at 118° C. to constant weight to obtain a steel for a hydraulic piston rod.

[0042] The smelting temperature in step S1 is 1480°C; the heat treatment in step S2 includes homogenization, normalizing, quenching and tempering in sequence; the homogenization temperature is 1180°C, and the holding time is 10 hours; the normalizing temperature is 900°C, and the holding time is 1.2 hours, followed by cooling in air; the quenching process is to keep at 870°C for 1.5 hours and then cool in water; the tempering process is to keep at 280°C for 1.5 hours and then cool in air.

[0043] The thickness of the functional coating in step S3 is 100 μm.

[0044] Example 3

[0045] A steel material for a hydraulic piston rod, comprising a steel material body and a functional coating covered on the surface thereof, wherein the steel material body comprises the following components in percentage by mass: C 0.350wt%, Si 0.32wt%, Mn 1.3wt%, Mo0.1wt%, Co 0.1wt%, Nb 0.08wt%, Cu 0.04wt%, rare earth elements 0.03wt%, Zr 0.035wt%, Ta0.02wt%, Os0.0025wt%, Ga 0.015wt%, Ti 0.04wt%, B 0.002wt%, N 0.0045wt%, nano titanium nitride 0.02wt%, nano chromium carbide 0.02wt%, and the rest are Fe and inevitable impurities; the functional coating is made of the following raw materials calculated by weight: 40 parts of hyperbranched perfluoropolyether polyurethane acrylate polymer, 2 parts of (perfluoropropane-2,2-diyl)bis(4,1-phenylene) diacrylate, 3 parts of bis(1-vinylimidazole-2-)ketone, 2 parts of 2-(1-propylene-2-yl)benzo[D]oxazole, 1 part of initiator, and 35 parts of solvent.

[0046] The rare earth element is a mixture of Sc, Y, Ce, and Gd in a mass ratio of 1:2:4:1; the particle size of the nano titanium nitride is 40 nm; the particle size of the nano chromium carbide is 60 nm; the hyperbranched perfluoropolyether polyurethane acrylate polymer is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN105482686B; the solvent is N-methylpyrrolidone; and the initiator is azobisisobutyronitrile.

[0047] A method for preparing the steel material for the hydraulic piston rod comprises the following steps:

[0048] Step S1, smelting raw materials Fe, C-Fe master alloy, Si-Fe master alloy, Mn-Fe master alloy, Mo-Fe master alloy, Co-Fe master alloy, Nb-Fe master alloy, Cu-Fe master alloy, rare earth element-Fe master alloy, Zr-Fe master alloy, Ta-Fe master alloy, Os-Fe master alloy, Ga-Fe master alloy, Ti-Fe master alloy, B-Fe master alloy, and N-Fe master alloy in a vacuum induction furnace, stirring to make the alloy composition uniform, then doping nano-titanium nitride and nano-chromium carbide preheated to 550-650° C. into the smelted alloy melt, and then stirring to make the composition uniform, and the alloy melt after stirring and doping is fully allowed to stand and then cast to obtain an ingot;

[0049] Step S2, sequentially heat treating, polishing, grinding, stamping, and turning the ingot produced in step S1 to obtain a steel body;

[0050] Step S3: After mixing the raw materials of the functional coating evenly, apply the mixture on the surface of the steel body, cure at 65° C. for 1.5 hours, and then dry at 120° C. to constant weight to obtain a steel for a hydraulic piston rod.

[0051] The smelting temperature in step S1 is 1510°C; the heat treatment in step S2 includes homogenization, normalizing, quenching and tempering in sequence; the homogenization temperature is 1210°C, and the holding time is 11h; the normalizing temperature is 910°C, and the holding time is 1.5h, followed by cooling in air; the quenching process is to keep at 875°C for 2 hours and then cool in water; the tempering process is to keep at 3050°C for 2 hours and then cool in air.

[0052] The thickness of the functional coating in step S3 is 100 μm.

[0053] Example 4

[0054] A steel material for a hydraulic piston rod, comprising a steel material body and a functional coating covered on the surface thereof, wherein the steel material body comprises the following components in percentage by mass: C 0.45wt%, Si 0.48wt%, Mn 1.5wt%, Mo0.13wt%, Co 0.11wt%, Nb 0.09wt%, Cu 0.05wt%, rare earth elements 0.04wt%, Zr 0.05wt%, Ta0.025wt%, Os0.0035wt%, Ga 0.018wt%, Ti 0.045wt%, B 0.0025wt%, N 0.0055wt%, nano titanium nitride 0.025wt%, nano chromium carbide 0.025wt%, the rest is Fe and inevitable impurities; the functional coating is made of the following raw materials calculated by weight: 45 parts of hyperbranched perfluoropolyether polyurethane acrylate polymer, 2.5 parts of (perfluoropropane-2,2-diyl)bis(4,1-phenylene) diacrylate, 3.5 parts of bis(1-vinylimidazole-2-)ketone, 2.5 parts of 2-(1-propylene-2-yl)benzo[D]oxazole, 1.1 parts of initiator, and 38 parts of solvent.

[0055] The rare earth element is a mixture of Sc, Y, Ce, and Gd in a mass ratio of 1:2:4.5:1; the particle size of the nano titanium nitride is 70 nm; the particle size of the nano chromium carbide is 80 nm; the hyperbranched perfluoropolyether polyurethane acrylate polymer is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN105482686B; the solvent is a mixture of N-methylpyrrolidone and N,N-dimethylformamide in a mass ratio of 3:5; and the initiator is azobisisobutyronitrile.

[0056] A method for preparing the steel material for the hydraulic piston rod comprises the following steps:

[0057] Step S1, smelting raw materials Fe, C-Fe master alloy, Si-Fe master alloy, Mn-Fe master alloy, Mo-Fe master alloy, Co-Fe master alloy, Nb-Fe master alloy, Cu-Fe master alloy, rare earth element-Fe master alloy, Zr-Fe master alloy, Ta-Fe master alloy, Os-Fe master alloy, Ga-Fe master alloy, Ti-Fe master alloy, B-Fe master alloy, and N-Fe master alloy in a vacuum induction furnace, stirring to make the alloy composition uniform, then doping nano-titanium nitride and nano-chromium carbide preheated to 640° C. into the smelted alloy melt, and then stirring to make the composition uniform, and the alloy melt after stirring and doping is fully allowed to stand and then cast to obtain an ingot;

[0058] Step S2, sequentially heat treating, polishing, grinding, stamping, and turning the ingot produced in step S1 to obtain a steel body;

[0059] Step S3: After mixing the raw materials of the functional coating evenly, apply the mixture on the surface of the steel body, cure at 68° C. for 1.8 hours, and then dry at 123° C. to constant weight to obtain a steel for a hydraulic piston rod.

[0060] The smelting temperature in step S1 is 1550°C; the heat treatment in step S2 includes homogenization, normalizing, quenching and tempering in sequence; the homogenization temperature is 1260°C, and the holding time is 12h; the normalizing temperature is 920°C, and the holding time is 1.8h, followed by cooling in air; the quenching process is to keep at 885°C for 2.5 hours and then cool in water; the tempering process is to keep at 330°C for 2.5 hours and then cool in air.

[0061] The thickness of the functional coating in step S3 is 100 μm.

[0062] Example 5

[0063] A steel material for a hydraulic piston rod, comprising a steel material body and a functional coating covered on the surface thereof, wherein the steel material body comprises the following components in percentage by mass: C 0.50wt%, Si 0.52wt%, Mn 1.6wt%, Mo0.15wt%, Co 0.12wt%, Nb 0.10wt%, Cu 0.06wt%, rare earth elements 0.05wt%, Zr 0.06wt%, Ta0.03wt%, Os0.004wt%, Ga 0.02wt%, Ti 0.05wt%, B 0.003wt%, N 0.006wt%, nano titanium nitride 0.03wt%, nano chromium carbide 0.03wt%, and the rest are Fe and inevitable impurities; the functional coating is made of the following raw materials calculated by weight: 50 parts of hyperbranched perfluoropolyether polyurethane acrylate polymer, 3 parts of (perfluoropropane-2,2-diyl)bis(4,1-phenylene) diacrylate, 4 parts of bis(1-vinylimidazole-2-)ketone, 3 parts of 2-(1-propylene-2-yl)benzo[D]oxazole, 1.2 parts of initiator, and 40 parts of solvent.

[0064] The rare earth element is a mixture of Sc, Y, Ce, and Gd in a mass ratio of 1:2:5:1; the particle size of the nano titanium nitride is 80 nm; the particle size of the nano chromium carbide is 90 nm; the hyperbranched perfluoropolyether polyurethane acrylate polymer is prepared according to the method of Example 1 of the Chinese invention patent with authorization announcement number CN105482686B; the solvent is N-methylpyrrolidone; and the initiator is azobisisobutyronitrile.

[0065] A method for preparing the steel material for the hydraulic piston rod comprises the following steps:

[0066] Step S1, smelting raw materials Fe, C-Fe master alloy, Si-Fe master alloy, Mn-Fe master alloy, Mo-Fe master alloy, Co-Fe master alloy, Nb-Fe master alloy, Cu-Fe master alloy, rare earth element-Fe master alloy, Zr-Fe master alloy, Ta-Fe master alloy, Os-Fe master alloy, Ga-Fe master alloy, Ti-Fe master alloy, B-Fe master alloy, and N-Fe master alloy in a vacuum induction furnace, stirring to make the alloy composition uniform, then doping nano-titanium nitride and nano-chromium carbide preheated to 650° C. into the smelted alloy melt, and then stirring to make the composition uniform, and the alloy melt after stirring and doping is fully allowed to stand and then cast to obtain an ingot;

[0067] Step S2, sequentially heat treating, polishing, grinding, stamping, and turning the ingot produced in step S1 to obtain a steel body;

[0068] Step S3: After mixing the raw materials of the functional coating evenly, apply the mixture on the surface of the steel body, cure at 70° C. for 2 hours, and then dry at 125° C. to constant weight to obtain a steel for a hydraulic piston rod.

[0069] The smelting temperature in step S1 is 1560°C; the heat treatment in step S2 includes homogenization, normalizing, quenching and tempering in sequence; the homogenization temperature is 1270°C, and the holding time is 13h; the normalizing temperature is 930°C, and the holding time is 2h, followed by cooling in air; the quenching process is to keep at 890°C for 3 hours and then water cool; the tempering process is to keep at 350°C for 3 hours and then cool in air.

[0070] The thickness of the functional coating in step S3 is 100 μm.

[0071] Comparative Example 1

[0072] A steel material for a hydraulic piston rod and a preparation method thereof are substantially the same as those of Example 1, except that Os, Ga, nano-titanium nitride and (perfluoropropane-2,2-diyl)bis(4,1-phenylene) diacrylate are not added.

[0073] Comparative Example 2

[0074] A steel material for a hydraulic piston rod and a preparation method thereof are substantially the same as those of Example 1, except that Ta, Co, nano-chromium carbide and bis(1-vinylimidazole-2-)ketone are not added.

[0075] In order to further illustrate the beneficial technical effects of the steel for hydraulic piston rods involved in each embodiment of the present invention, relevant performance tests were conducted on the steel for hydraulic piston rods involved in Examples 1-5 and Comparative Examples 1-2; the test method is as follows:

[0076] (1) Tensile strength: Tested in accordance with standard GB / T228-2002 “Room temperature tensile test method for metal materials”.

[0077] (2) Corrosion resistance: The prepared hydraulic piston rod steel is subjected to a salt spray corrosion test at a test temperature of 35°C. A 5% mass concentration sodium chloride aqueous solution is sprayed in the test chamber to simulate the accelerated corrosion environment. The corrosion-resistant gears are qualified if their tolerance time (i.e., the time they remain rust-free) exceeds 1500 hours; otherwise, they are unqualified.

[0078] (3) Wear resistance: The friction and wear test of each hydraulic piston rod steel body sample was carried out using a MFT-R4000 high-speed reciprocating friction and wear tester. The test load was 30N, the test time was 5min, and the friction length was 5×10 -3 m, the friction ball is The Al2O3 material is used to measure the wear mass and obtain the wear rate by calculation. The wear rate W is calculated using the following formula: W = m / N·L, where W is the wear rate (g / N·m); m is the wear mass (g); N is the load (N); and L is the total stroke (m).

[0079] (4) Fatigue resistance: The specimens were subjected to a constant amplitude fatigue test (maximum load 100 MPa, minimum load 20 MPa) on an Amsler HFP-422 high frequency fatigue testing machine, and the fatigue life was recorded and counted.

[0080] As can be seen from Table 1, the steel for hydraulic piston rod involved in each embodiment of the present invention has better mechanical properties, wear resistance, corrosion resistance and fatigue resistance than the comparative product, and the combined use of Os, Ga, nano-titanium nitride, (perfluoropropane-2,2-diyl)bis(4,1-phenylene) diacrylate, Ta, Co, nano-chromium carbide and bis(1-vinylimidazole-2-)ketone is beneficial to improving the above properties.

[0081] Table 1

[0082] project tensile strength Wear rate Corrosion resistance Fatigue life unit MPa <![CDATA[×10 -10 g / N·m]]> — Ten thousand times Example 1 1200 0.15 qualified 16.3 Example 2 1211 0.12 qualified 16.5 Example 3 1220 0.10 qualified 16.8 Example 4 1234 0.08 qualified 16.9 Example 5 1242 0.07 qualified 17.1 Comparative Example 1 1125 0.21 Failure 15.2 Comparative Example 2 1109 0.23 Failure 14.8

[0083] The above embodiments are only for illustrating the technical concept and features of the present invention, and their purpose is to enable people familiar with this technology to understand the contents of the present invention and implement them accordingly. They cannot be used to limit the protection scope of the present invention. All equivalent changes or modifications made according to the spirit of the present invention should be included in the protection scope of the present invention.

Claims

1. A steel material for a hydraulic piston rod, characterized in that: The invention comprises a steel body and a functional coating covered on the surface thereof, wherein the steel body comprises the following components in percentage by mass: C 0.15-0.50wt%, Si 0.12-0.52wt%, Mn 1.0-1.6wt%, Mo 0.05-0.15wt%, Co 0.08-0.12wt%, Nb 0.06-0.10wt%, Cu 0.01-0.06wt%, rare earth elements 0.01-0.05wt%, Zr 0.01-0.06wt%, Ta 0.01-0.03wt%, Os0.001-0.004wt%, Ga0.01-0.02wt%, Ti 0.03-0.05wt%, B 0.001-0.003wt%, N The functional coating is prepared from the following raw materials calculated in parts by weight: 30-50 parts of hyperbranched perfluoropolyether polyurethane acrylate oligomer, 1-3 parts of (perfluoropropane-2,2-diyl)bis(4,1-phenylene) diacrylate, 2-4 parts of bis(1-vinylimidazole-2-)ketone, 1-3 parts of 2-(1-propylene-2-yl)benzo[D]oxazole, 0.8-1.2 parts of initiator, and 30-40 parts of solvent.

2. The steel material for hydraulic piston rod according to claim 1, characterized in that: The rare earth elements are a mixture of Sc, Y, Ce and Gd in a mass ratio of 1:2:(3-5):

1.

3. The steel material for hydraulic piston rod according to claim 1, characterized in that: The particle size of the nano titanium nitride is 10-80 nm; the particle size of the nano chromium carbide is 20-90 nm.

4. The steel material for hydraulic piston rod according to claim 1, characterized in that: The solvent is at least one of N-methylpyrrolidone and N,N-dimethylformamide; and the initiator is azobisisobutyronitrile.

5. A method for preparing the steel material for hydraulic piston rod according to any one of claims 1 to 4, characterized in that: The steps include: Step S1, smelting raw materials Fe, C-Fe master alloy, Si-Fe master alloy, Mn-Fe master alloy, Mo-Fe master alloy, Co-Fe master alloy, Nb-Fe master alloy, Cu-Fe master alloy, rare earth element-Fe master alloy, Zr-Fe master alloy, Ta-Fe master alloy, Os-Fe master alloy, Ga-Fe master alloy, Ti-Fe master alloy, B-Fe master alloy, and N-Fe master alloy in a vacuum induction furnace, stirring to make the alloy composition uniform, then doping nano-titanium nitride and nano-chromium carbide preheated to 550-650° C. into the smelted alloy melt, and then stirring to make the composition uniform, and the stirred and doped alloy melt is fully allowed to stand before pouring to obtain an ingot; Step S2, sequentially heat treating, polishing, grinding, stamping, and turning the ingot produced in step S1 to obtain a steel body; Step S3: After uniformly mixing the raw materials of the functional coating, apply the mixture on the surface of the steel body, cure at 60-70°C for 1-2 hours, and then dry at 115-125°C to constant weight to obtain a steel material for a hydraulic piston rod.

6. The method for preparing a steel material for a hydraulic piston rod according to claim 5, characterized in that: The smelting temperature in step S1 is 1450-1560°C.

7. The method for preparing a steel material for a hydraulic piston rod according to claim 5, characterized in that: The heat treatment in step S2 includes homogenization treatment, normalizing treatment, quenching treatment and tempering treatment performed in sequence.

8. The method for preparing a steel material for a hydraulic piston rod according to claim 7, characterized in that: The temperature of the homogenization treatment is 1160-1270° C., and the holding time is 8-13 hours.

9. The method for preparing a steel material for a hydraulic piston rod according to claim 7, characterized in that: The normalizing treatment temperature is 880-930°C, the holding time is 1-2 hours, and then cooling in air; the quenching treatment process is to keep the temperature at 860-890°C for 1-3 hours and then water-cool; the tempering treatment process is to keep the temperature at 250-350°C for 1-3 hours and then cool in air.

10. The method for preparing a steel material for a hydraulic piston rod according to claim 5, characterized in that: The thickness of the functional coating in step S3 is 50-160 μm.

Citation Information

Patent Citations

  • Preparation method of wear-resistant composite coating on surface of automobile body steel plate

    CN112941511A

  • Processing technology of corrosion-resistant stainless steel pipe for conveying catalyst

    CN113308692A

  • High-toughness cast steel and production method thereof

    CN116377336A

  • Low alloy high performance steel

    US20160369362A1

  • Martensitic heat-resistant steel for use at 630ºc or more and preparation method therefor

    WO2023246465A1