Anti-cleavage martensite ultrahigh-strength steel and preparation method thereof

By accurately controlling the C, Cr, Mo, Ni, and Co element content in ultra-high strength steel and adopting specific process processing, the problems of high cost and strong resource dependence in the existing technology are solved, and a low cost is developed The cleavage-resistant martensite ultra-high strength steel with high tensile strength has achieved similar performance to the existing secondary hardened ultra-high strength steel but significantly reduced alloy element content.

CN119082622AActive Publication Date: 2024-12-06CHINA IRON & STEEL RESEARCH INSTITUTE GROUP CO LTD
View PDF 4 Cites 0 Cited by

Patent Information

Application Number
CN202411199861.7
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06
Estimated Expiration
2044-08-29

AI Technical Summary

Technical Problem

The production cost of existing secondary hardening ultra-high strength steel above 2000MPa grade is too high, and the resource dependence is strong, making it difficult to achieve large-scale industrial application.

Method used

Chemical composition of cleavage-resistant martensite ultra-high strength steel, including C 0.35-0.50%, Cr 1-5%, Mo 0.5-3%, Ni 2-9%, Co 1-8%, by precise control of elements Content and process treatment, ultra-high strength steel with excellent tensile strength and fracture toughness were prepared, including smelting, normalizing, annealing, quenching, deep-cooling and low-temperature tempering treatment.

Benefits of technology

Achieve ultra-high strength steel with low cost and tensile strength exceeding 2200MPa, which reduces the alloy element content and significantly reduces production costs. At the same time, it maintains excellent tensile strength and fracture toughness, with an elongation of more than 11%, and a cross-sectional shrinkage rate greater than 40%, the fracture toughness KIC is greater than 65MPa·m1/2.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure SMS_1
    Figure SMS_1
  • Figure SMS_2
    Figure SMS_2
Patent Text Reader

Abstract

The invention relates to the technical field of metal smelting, and particularly discloses cleavage-resistant martensite ultrahigh-strength steel and a preparation method thereof. The anti-cleavage martensite ultra-high-strength steel is disclosed. The invention relates to a high-temperature-resistant steel wire rope which comprises the following chemical components in percentage by weight: 0.35-0.50% of 1-5% of Cr; 0.5 to 3% of Mo; 2-9% of Ni; 1-8% of Co; the balance is Fe and inevitable impurities; and the Ni content is 1-5% higher than the Co content. The 2200MPa-grade ultra-high-strength steel which is low in cost and has excellent strength and toughness is developed aiming at the problems that the cost of existing 2,000 MPa-grade or above secondary hardening type ultra-high-strength steel is too high, and the resource dependence is too high.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present application relates to the technical field of metal smelting, and more specifically, to a cleavage-resistant martensitic ultra-high strength steel and a preparation method thereof. Background Art

[0002] Ultra-high strength steel is widely used in key load-bearing components such as aerospace, energy and transportation, and weapons and equipment. It is often subjected to cyclic loads during service. Therefore, the fatigue performance of ultra-high strength steel is particularly important for its service safety and reliability. Studies have shown that when the strength grade of steel materials is low, its fatigue performance is positively correlated with tensile strength, while when the strength grade of steel materials is above 1800-2000MPa, its fatigue performance decreases with the increase of strength. Therefore, the fatigue resistance of steel materials under ultra-high strength needs to comprehensively consider the matching relationship between strength and toughness, especially strength and fracture toughness.

[0003] Due to its excellent strength and toughness, secondary hardening ultra-high strength steel has been widely used. Representative products are the American Aermet series of secondary hardening ultra-high strength steels, such as Aermet100, which has a tensile strength of 1960MPa and a plane strain fracture toughness (K IC ) greater than 110MPa·m 1 / 2 ; Aermet310 has a tensile strength of 2170MPa, K IC Up to 70MPa·m 1 / 2 The chemical composition of typical secondary hardening ultra-high strength steel is shown in Table 1. However, the addition of more than 25% of alloying elements greatly increases the production cost of this type of secondary hardening ultra-high strength steel, restricting its large-scale industrial application.

[0004] Table 1 Chemical composition of typical secondary hardening ultra-high strength steel

[0005]

[0006] Therefore, there is an urgent need to develop an ultra-high strength steel with low cost and a tensile strength of more than 2200 MPa, while having both excellent strength and toughness. Summary of the invention

[0007] In view of the high cost and resource dependence of the existing secondary hardening ultra-high strength steel of 2000MPa or above, the present application develops an ultra-high strength steel of 2200MPa or above with low cost and excellent strength and toughness. The present application provides a cleavage-resistant martensitic ultra-high strength steel and a preparation method thereof.

[0008] In a first aspect, the present application provides a cleavage-resistant martensitic ultra-high strength steel, which adopts the following technical solution:

[0009] A cleavage-resistant martensitic ultra-high strength steel comprises, by weight percentage, the chemical composition of the cleavage-resistant martensitic ultra-high strength steel: C 0.35-0.50%, Cr 1-5%, Mo 0.5-3%, Ni 2-9%, Co 1-8%, and the balance being Fe and unavoidable impurities.

[0010] Optionally, in the chemical composition of the cleavage-resistant martensitic ultra-high strength steel, the Ni content is 1-5% higher than the Co content.

[0011] Optionally, the ultra-high strength steel has a tensile strength of ≥2200 MPa and a fracture toughness of ≥65 MPa·m 1 / 2 .

[0012] In a second aspect, the present application provides a method for preparing cleavage-resistant martensitic ultra-high strength steel, which adopts the following technical solution:

[0013] A method for preparing cleavage-resistant martensitic ultra-high strength steel comprises smelting, normalizing treatment, annealing treatment, quenching treatment, deep cryogenic treatment and low-temperature tempering treatment.

[0014] Furthermore, the smelting is to prepare ultra-high strength steel having a chemical composition within the required range using methods including but not limited to a converter, an electric furnace, a vacuum induction furnace, an LF furnace, a vacuum consumable method or a combination of two or more of the above methods.

[0015] Furthermore, the normalizing treatment includes heating the rod to 910-960° C., keeping the temperature for 1-3 hours, and air cooling to room temperature.

[0016] Furthermore, the annealing treatment includes heating the rod to 620-680° C., keeping the temperature for 6-15 hours, and air cooling to room temperature.

[0017] Furthermore, the quenching treatment includes heating the rod to 900-960° C., keeping the temperature for 1-2 hours, and oil cooling.

[0018] Furthermore, the cryogenic treatment includes subjecting the rod to cryogenic treatment in the range of (-196)-(-73)°C, keeping the temperature for 0.5-3h, and air cooling to room temperature.

[0019] Furthermore, the low temperature tempering treatment includes heating the rod to 120-200° C., keeping the temperature for 1-6 hours, and air cooling to room temperature.

[0020] In a specific embodiment, a method for preparing cleavage-resistant martensitic ultra-high strength steel comprises the following steps:

[0021] (1) Melting: Ultra-high strength steel with chemical composition within the required range is prepared by using, but not limited to, converters, electric furnaces, vacuum induction furnaces, LF furnaces, vacuum consumable methods, or a combination of two or more of the above methods.

[0022] (2) Normalizing: Heat the bar to 910-960℃, keep warm for 1-3h, and air cool to room temperature.

[0023] (3) Annealing: Heat the bar to 620-680℃, keep it warm for 6-15h, and air cool it to room temperature.

[0024] (4) Quenching treatment: Heat the bar to 900-960℃, keep warm for 1-2h, and oil cool.

[0025] (5) Cryogenic treatment: Cryogenic treatment of the bar in the range of (-196)-(-73)℃, keep warm for 0.5-3h, and air cool to room temperature.

[0026] (6) Low temperature tempering treatment: Heat the bar to 120-200℃, keep warm for 1-6h, and air cool to room temperature.

[0027] In summary, this application has the following beneficial effects:

[0028] In response to the problems of high cost and strong resource dependence of existing secondary hardening ultra-high strength steel above 2000MPa, this application develops an ultra-high strength steel above 2200MPa that is low in cost and has excellent strength and toughness.

[0029] The cleavage-resistant martensitic ultra-high strength steel provided in the present application is prepared by precisely controlling the contents of C, Cr, Mo, Ni, and Co elements in the ultra-high strength steel, obtaining a tempered martensitic matrix structure and a high-density nanoscale ε precipitation phase through a process of quenching + deep cooling + low-temperature tempering, using 2-9% of Ni elements to toughen the martensitic matrix, using 1-8% of Co elements to regulate the Ms point and improve the strength and tempering resistance, and controlling the Ni content to be 2-5% higher than the Co content to synergistically regulate the material properties, while having good tensile strength and toughness and plasticity.

[0030] The cleavage-resistant martensitic ultra-high strength steel provided in the present application has excellent performance, with a tensile strength of more than 2200 MPa, an elongation greater than 11%, a cross-sectional shrinkage greater than 40%, and a fracture toughness K IC Greater than 65MPa·m 1 / 2 Compared with the existing secondary hardening ultra-high strength steel of the same strength grade, the tensile strength and fracture toughness are basically the same, but the alloying element content is significantly reduced, and the alloying cost is greatly reduced. DETAILED DESCRIPTION

[0031] Before describing the embodiments of the present application in detail, it should be understood that the terms used herein are only used for the purpose of describing specific embodiments. Unless otherwise defined, all technical and scientific terms used herein have the same meaning as those generally understood by ordinary technicians in the field to which the terms belong.

[0032] The present application provides a cleavage-resistant martensitic ultra-high strength steel, which comprises, by weight percentage, 0.35-0.50% C, 1-5% Cr, 0.5-3% Mo, 2-9% Ni, 1-8% Co, and the remainder Fe and unavoidable impurities.

[0033] Furthermore, in terms of weight percentage, in its chemical composition, the Ni content is 1-5% higher than the Co content.

[0034] The following is a detailed description of the chemical components and dosage selection of the cleavage-resistant martensitic ultra-high strength steel of the present application.

[0035] In terms of weight percentage, the ultra-high strength steel of the present application includes C 0.35-0.50%. In the present application, the C element is the most important strengthening element. The C element content directly determines the strength of martensite. Controlling the C content above 0.35% is the key to ensuring the strength of the material. However, too high a C content (> 0.50%) will significantly deteriorate the toughness and plasticity of the material, especially damage the fracture toughness. Therefore, the C content in the ultra-high strength steel of the present application is controlled to be 0.35-0.50%.

[0036] In terms of weight percentage, the ultra-high strength steel of the present application includes Cr 1-5%. In the present application, the Cr element can improve the strength of the steel by solid solution strengthening and precipitation strengthening, while improving the hardenability and tempering resistance of the steel. However, too high a Cr content will significantly reduce the Ms point (starting temperature of martensitic transformation) of the steel, resulting in too much residual austenite, and at the same time, it is easy to have Cr-containing carbides with too high precipitation temperature before solution treatment, thereby increasing the solid solution temperature, resulting in coarse grains and tissues. Therefore, the Cr content in the ultra-high strength steel of the present application is controlled to be 1-5%.

[0037] In terms of weight percentage, the ultra-high strength steel of the present application includes 0.5-3% Mo. In the present application, the Mo element can improve the strength of the steel, improve the hardenability and tempering resistance, and inhibit the effect of tempering brittleness. However, too high a Mo content will increase the quenching temperature. Therefore, the Mo content in the ultra-high strength steel of the present application is controlled to be 0.5-3%.

[0038] In terms of weight percentage, the ultra-high strength steel of the present application includes Ni 2-9%. In the present application, Ni element is the main toughening element, and Ni element can improve the resistance of the martensite matrix to cleavage fracture to ensure sufficient toughness. However, too high Ni content will significantly reduce the Ms point of the steel, resulting in the formation of excessive and blocky residual austenite, which will damage the toughness of the steel. Therefore, the Ni content in the ultra-high strength steel of the present application is controlled to be 2-9%.

[0039] In terms of weight percentage, the ultra-high strength steel of the present application includes Co 1-8%. In the present application, the Co element is the main element to increase the Ms point. By adding Co, the Ms point of the steel is regulated to a reasonable range, thereby avoiding the formation of too much residual austenite. Co can also delay the dislocation recovery in the martensitic matrix during tempering and improve the tempering resistance. However, too high a Co content will damage the toughness of the steel. Therefore, the Co content in the ultra-high strength steel of the present application is controlled to be 1-8%.

[0040] In terms of weight percentage, the present application requires that the Ni content be 1-5% higher than the Co content. The combination of Ni and Co content can adjust the Ms point to a reasonable range to avoid the formation of excessive residual austenite. The addition of Co can also compensate for the reduction in strength caused by Ni. At the same time, Co can significantly improve the tempering resistance and avoid the tempering temperature of the steel being too low. Therefore, the ultra-high strength steel of the present application requires that the Ni content be 1-5% higher than the Co content.

[0041] The ultra-high strength steel of the present application also includes inevitable impurity elements. The impurity elements mainly include S, P, O, N, H, Al, Ti, etc. Further, in terms of weight percentage, S≤0.003%, P≤0.005%, S≤0.003%, O≤0.003%, N≤0.003%, H≤0.00002%, Al≤0.03%, Ti≤0.01%. The present application controls the impurity elements within the above range to ensure the toughness and fatigue life of the material.

[0042] To make the purpose, technical solutions and advantages of this application clearer, the technical solutions in the embodiments of this application are described clearly and completely below. Based on the embodiments of this application, all other embodiments obtained by those skilled in the art without creative work are within the scope of protection of this application.

[0043] The present application is further described in detail below in combination with embodiments, comparative examples and test results.

[0044] Example

[0045] Example 1

[0046] This embodiment provides a cleavage-resistant martensitic ultra-high strength steel. The chemical composition of the ultra-high strength steel is shown in Table 2.

[0047] The preparation method of the above-mentioned cleavage-resistant martensitic ultra-high strength steel is specifically as follows:

[0048] (1) Melting: Ultra-high strength steel with chemical composition within the required range is prepared using a vacuum consumable method.

[0049] (2) Normalizing: Heat the bar to 950°C, keep warm for 1 hour, and air cool to room temperature.

[0050] (3) Annealing: Heat the bar to 660°C, keep it at this temperature for 8 h, and air cool it to room temperature.

[0051] (4) Quenching treatment: heat the bar to 950℃, keep warm for 1h, and cool with oil.

[0052] (5) Cryogenic treatment: Cryogenically treat the bar at (-73) °C, keep warm for 2 h, and air cool to room temperature.

[0053] (6) Low temperature tempering treatment: Heat the bar to 170℃, keep it warm for 1h, and air cool it to room temperature.

[0054] Table 2 Chemical composition and mechanical properties of ultra-high strength steel provided in the examples and comparative examples

[0055]

[0056] Example 2-3

[0057] Examples 2-3 provide a cleavage-resistant martensitic ultra-high strength steel respectively. The above ultra-high strength steel is different from Example 1 in that the content of Ni and Co and the low-temperature tempering temperature are specifically shown in Table 2. The remaining operation steps are consistent with Example 1.

[0058] Comparative Example

[0059] Comparative Example 1

[0060] Comparative Example 1 provides a cleavage-resistant martensitic ultra-high strength steel. The difference between the ultra-high strength steel and Example 1 is that the Ni content is about 6% higher than the Co content, as shown in Table 2. The remaining operation steps are consistent with Example 1.

[0061] Comparative Examples 2-3

[0062] Comparative Examples 2-3 provide a cleavage-resistant martensitic ultra-high strength steel respectively. The above ultra-high strength steel is different from Example 1 in that the Co content is 0 and the low-temperature tempering temperature is shown in Table 2. The remaining operation steps are consistent with Example 1.

[0063] Performance test results

[0064] The following mechanical property tests were performed on the ultra-high strength steel provided in the above examples and comparative examples, as well as AF1410 (510° C. aging treatment for 5 h) and Aermet100 (482° C. aging treatment for 5 h). The test results are shown in Table 2.

[0065] Among them, the test methods for tensile strength, yield strength, elongation and cross-sectional shrinkage refer to GB / T 228.1-2010, and the test method for fracture toughness refers to GB / T 4161-2007.

[0066] As shown in Table 2, according to the test results of Examples 1-3, the tensile strength of the ultra-high strength steel provided in this application is ≥2200MPa, and the fracture toughness is ≥65MPa·m 1 / 2 In Comparative Example 1, the Ni content is about 6% higher than the Co content. At this time, the tensile strength of the ultra-high strength steel provided by Comparative Example 1 is close to 2200MPa, while the fracture toughness is only 59MPa·m 1 / 2 From Comparative Examples 2-3, it can be seen that in the absence of Co, after tempering at 120°C and 150°C, although the tensile strength of the ultra-high strength steel meets ≥2200MPa, the fracture toughness is only 50.01MPa·m 1 / 2 and 60.7MPa·m 1 / 2 The tensile strengths of AF1410 (aged at 510℃ for 5h) and Aermet100 (aged at 482℃ for 5h) are both lower than 2000MPa.

[0067] Finally, it should be noted that the above embodiments are only used to illustrate the technical solutions of the present application, rather than to limit it. Although the present application has been described in detail with reference to the aforementioned embodiments, those skilled in the art should understand that they can still modify the technical solutions described in the aforementioned embodiments, or make equivalent replacements for some of the technical features therein. However, these modifications or replacements do not deviate the essence of the corresponding technical solutions from the spirit and scope of the technical solutions of the embodiments of the present application.

Claims

1. A cleavage-resistant martensitic ultra-high strength steel, characterized in that: The chemical composition of the cleavage-resistant martensitic ultra-high-strength steel includes, by weight percentage: C 0.35-0.50%; Cr 1-5%; Mo 0.5-3%; Ni 2-9%; Co 1-8%; the remainder is Fe and unavoidable impurities; in the chemical composition of the cleavage-resistant martensitic ultra-high-strength steel, the Ni content is 1-5% higher than the Co content.

2. The cleavage-resistant martensitic ultra-high strength steel according to claim 1, characterized in that: The tensile strength of the ultra-high strength steel is ≥2200MPa, and the fracture toughness is ≥65MPa·m 1 / 2 .

3. A method for preparing cleavage-resistant martensitic ultra-high strength steel, characterized in that: The preparation method comprises smelting, normalizing treatment, annealing treatment, quenching treatment, deep freezing treatment and low-temperature tempering treatment.

4. The preparation method according to claim 3, characterized in that: The smelting is to prepare ultra-high strength steel with chemical composition within the required range by using, but not limited to, a converter, an electric furnace, a vacuum induction furnace, an LF furnace, a vacuum consumable method or a combination of two or more of the above methods.

5. The preparation method according to claim 3, characterized in that: The normalizing treatment includes heating the rod to 910-960° C., keeping the temperature for 1-3 hours, and air cooling to room temperature.

6. The preparation method according to claim 3, characterized in that: The annealing treatment includes heating the rod to 620-680° C., keeping the temperature for 6-15 hours, and air cooling to room temperature.

7. The preparation method according to claim 3, characterized in that: The quenching treatment includes heating the rod to 900-960° C., keeping the temperature for 1-2 hours, and oil cooling.

8. The preparation method according to claim 3, characterized in that: The cryogenic treatment includes subjecting the rod to cryogenic treatment in the range of (-196)-(-73)°C, keeping the temperature for 0.5-3h, and air cooling to room temperature.

9. The preparation method according to claim 3, characterized in that: The low temperature tempering treatment includes heating the rod to 120-200° C., keeping the temperature for 1-6 hours, and air cooling to room temperature.

Citation Information

Patent Citations

  • 10Ni10Co high-toughness secondary-hardening ultrahigh-strength steel and preparation method thereof

    CN104073736A

  • Economical high-toughness ultrahigh-strength steel and preparation method thereof

    CN116288067A

  • Ultra high strength steel having low yield ratio and its manufacture

    JP1989242761A

  • Maraging steel and method for manufacturing same

    US20200071804A1