High-strength and high-toughness microalloy structural steel and preparation method thereof
By depositing a modified graphite layer on the surface of microalloy structural steel, combined with high-temperature and low-temperature carburizing processes, the problems of coarse grains and long precarburizing time of microalloy structural steel are solved, and high strength, toughness and high-efficiency carburizing effects are achieved.
Patent Information
- Application Number
- CN202411216237.3
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-09-02
- Publication Date
- 2024-12-06
- Estimated Expiration
- 2044-09-02
AI Technical Summary
Microalloy structural steels are prone to coarse grains in conventional carburizing processes, resulting in a decrease in strength or toughness, and the precarburizing step is too long, which affects efficiency.
Using a combination of high-temperature carburizing and low-temperature carburizing, by depositing a modified graphite layer on the surface of the steel matrix, using modified graphite as the carbide growth core, high-temperature carburizing is directly carried out, and carbides are further refined at low temperatures to reduce the Stress within the carburizing layer to optimize the uniformity of the carburizing layer.
It effectively improves the strength and toughness of microalloy structural steel, avoids the problem of coarse grains, simplifies the process flow, and improves carburizing efficiency and performance.
Smart Images

Figure BDA0005021605560000111
Abstract
Description
Technical Field
[0001] The invention relates to the field of alloy structural steel, and specifically discloses a high-strength and toughness microalloy structural steel and a preparation method thereof. Background Art
[0002] Microalloy structural steel has good performance and is widely used in bridges, high-rise buildings, power generation equipment, various pipelines and other fields. The amount of alloying elements added to the steel matrix is very small, but it can significantly improve the performance. Microalloying in the steel matrix plays a role in grain refinement, reducing inclusions, reducing cracks, and improving hardenability. The appropriate type and content of alloying elements can be determined according to specific needs.
[0003] Carburizing the surface of microalloyed structural steel can further improve its strength, but the conventional carburizing process will lead to coarse grains, and the pre-carburizing step takes too long. The above problems will lead to a certain degree of decrease in the strength or toughness of microalloyed structural steel; therefore, it is of great significance to study a high-strength and toughness microalloyed structural steel and its preparation method. Summary of the invention
[0004] The object of the present invention is to provide a high-strength and toughness microalloy structural steel and a preparation method thereof to solve the problems raised in the above background technology.
[0005] In order to solve the above technical problems, the present invention provides the following technical solutions: A method for preparing high-strength and high-toughness microalloy structural steel comprises the following steps:
[0006] S1: adding a refining agent to the molten iron, refining and slag removal; adding a modifier, modifying treatment; vacuum degassing, continuous casting, rolling in sequence to obtain basic structural steel;
[0007] S2: The basic structural steel is cleaned and electroplated to obtain structural steel A with modified graphite deposited on the surface;
[0008] S3: Take structural steel A, perform high temperature carburizing, low temperature carburizing, diffusion, quenching cooling, and tempering to obtain high strength and toughness microalloy structural steel.
[0009] More optimally, step S1 specifically includes: taking molten iron; adding 1-2% of the mass of the molten iron refining agent at 1600-1700°C, stopping for 20-30 minutes, and then slagging; adding 1-2% of the mass of the molten iron modifier, staying for 20-30 minutes, and removing the slag; performing vacuum degassing, continuous casting (temperature: 1180-1220°C), and rolling (heating at 1200°C for 5-6 hours and then rolling to open the blank, pit cooling to 180°C after opening the blank, and then heating to 1180°C again, keeping warm for 5-6 hours, and rolling after the end of the insulation, the initial rolling temperature is 1100-1180°C, the final rolling temperature is 850-1000°C, and air cooling is performed after rolling) to obtain basic structural steel.
[0010] More optimally, step S1 specifically includes: taking molten iron; adding a refining agent of 1% by mass of the molten iron at 1600°C, stopping for 20 minutes, and then slagging; adding a modifier of 1% by mass of the molten iron, stopping for 25 minutes, and then removing the slag; performing vacuum degassing, continuous casting (temperature: 1220°C), and rolling (heating at 1200°C for 6 hours and then rolling to open the blanks, pit cooling to 180°C after opening the blanks, and then heating to 1180°C again, keeping warm for 6 hours, and then rolling after the end of the insulation, the initial rolling temperature is 1100°C, the final rolling temperature is 950°C, and air cooling is performed after rolling) to obtain basic structural steel.
[0011] More optimally, the molten iron includes the following components in percentage by mass: C: 0.7-0.85%, Si: 0.15-0.35%, Mn: 0.70-0.90%, P: ≤0.025%, S: ≤0.025%, Cr: 0.16-0.25%, V: 0.068-0.08%, Cu: ≤0.001%, Ni: ≤0.001%, Ti: ≤0.001%, and the rest are Fe and unavoidable impurities.
[0012] More optimally, the molten iron includes the following components in percentage by mass: C: 0.75%, Si: 0.2%, Mn: 0.75%, P: 0.005%, S: 0.015%, Cr: 0.22%, V: 0.071%, Cu: 0.001%, Ni: 0.001%, Ti: 0.001%, and the rest is Fe and unavoidable impurities.
[0013] More optimally, the cleaning process in step S2 is: clean the basic structural steel with 80° C. water for 30 seconds, immerse in 5% sulfuric acid for 10 minutes, and then rinse with water.
[0014] More optimally, the specific process of electroplating in step S2 is: controlling the temperature to 50-60°C, pH to 7-8, and the current density to 4-6A / dm 3 , electroplating in the electroplating solution for 10 to 15 minutes;
[0015] The electroplating solution includes the following raw materials: 30-40 g / L nickel sulfate hexahydrate, 5-15 g / L nickel chloride hexahydrate, 5-10 g / L zinc sulfate, 3.5-10.5 g / L titanyl sulfate, 50-60 g / L trisodium citrate, 5-10 g / L additives, 5-10 g / L modified graphite, and the rest is water.
[0016] More optimally, the preparation of the modified graphite includes the following steps: Step 1: Take epoxy silane coupling agent, di(hydroxyethyl)methyl dodecyl ammonium chloride, 3-amino-5-fluoropyridine, and DMSO, heat to 130-140° C., stir for 4-6 hours, remove the solvent, and obtain modifier A;
[0017] Step 2: Take nanographite, ethanol, and water, add modifier A, stir at 40-50° C. for 5-6 hours, filter, and dry to obtain modified graphite;
[0018] The modifier A comprises the following raw materials, calculated by weight: 10 to 15 parts of epoxy silane coupling agent, 5 to 8 parts of di(hydroxyethyl)methyl dodecyl ammonium chloride, 2 to 4 parts of 3-amino-5-fluoropyridine, and 150 to 200 parts of DMSO;
[0019] The modified graphite comprises the following raw materials, calculated by weight: 10 to 15 parts of nanographite, 40 to 60 parts of ethanol, 40 to 60 parts of water, and 3 to 5 parts of modifier A.
[0020] More optimally, the preparation of the additive includes the following steps: Step 1: Take portions of hyperbranched polyacrylic acid, citrate, 6-hydroxy-2-pyridinecarboxylic acid, stannous isooctanoate, and p-toluenesulfonic acid monohydrate, mix them evenly, heat to 130-140° C. and stir for 1-2 hours, heat to 150-160° C. and stir for 4-6 hours, cool to 130-140° C., add epoxy silane coupling agent, stir for 4-6 hours, remove the solvent, and obtain modifier B;
[0021] Step 2: Take molybdenum disulfide, ethanol, and water, add modifier B, and stir at 40-50° C. for 5-6 hours to obtain an additive;
[0022] The modifier B comprises the following raw materials, calculated by mass: 15 to 20 parts of hyperbranched polyacrylic acid, 4 to 6 parts of citrate, 1 to 3 parts of 6-hydroxy-2-pyridinecarboxylic acid, 0.1 to 0.2 parts of stannous isooctanoate, 0.04 to 0.05 parts of p-toluenesulfonic acid monohydrate, and 10 to 15 parts of epoxy silane coupling agent;
[0023] The additive comprises the following raw materials, calculated by weight: 5 to 10 parts of molybdenum disulfide, 40 to 60 parts of ethanol, 40 to 60 parts of water, and 8 to 12 parts of modifier B.
[0024] More optimally, in step S2, the specific process of high-temperature carburizing is as follows: temperature is 900-950°C, carbon potential is 1.1, and time is 3-4h; the specific process of low-temperature carburizing is as follows: temperature is 800-850°C, carbon potential is 1.1, and time is 2-3h; the specific process of diffusion is as follows: temperature is 800-850°C, carbon potential is 0.8, and time is 1-2h.
[0025] More optimally, the refining agent includes the following raw materials, by mass percentage: 80-90% CaO, 10-20% Al2O3; the modifier includes the following raw materials, by mass percentage: 50-60% rare earth ferrosilicon, 20-30% modified ferrosilicon, 10-20% silicon-calcium alloy, 5-10% trace elements; the trace elements include the following raw materials, by mass percentage: 40% Zr, 25% Cu, 15% Sb, 15% Bi and 5% B.
[0026] More optimally, the refining agent includes the following raw materials, by mass percentage: 85% CaO, 15% Al2O3.
[0027] More optimally, the preparation of the modified ferrosilicon includes the following steps: mixing titanium carbide powder and nickel-based powder in a mass ratio of (1-2):1 to obtain a mixture; and depositing the mixture on the surface of ferrosilicon by plasma transfer arc welding to obtain modified ferrosilicon.
[0028] More optimally, the preparation of the modified ferrosilicon includes the following steps: mixing titanium carbide powder and nickel-based powder in a mass ratio of 2:1 to obtain a mixture; the mixture is deposited on the surface of ferrosilicon by plasma transfer arc welding to obtain modified ferrosilicon; the nickel-based powder is METCOCLAD 625 powder (Ni21Cr9Mo4Nb) of Oerlikon Metco; the deposition equipment is STARWELD 400A with an EXCALIBUR welding torch, and the deposition parameters are: 2L / minAr center gas flow, 2L / minAr powder gas flow, 12L / minAr shielding gas flow, voltage 29V, current 145A, and deposition time 0.2s.
[0029] Compared with the prior art, the beneficial effects achieved by the present invention are as follows: after the slag removal is completed, a modifier is added to further refine the grains, and the modifier contains modified ferrosilicon, that is, ferrosilicon of titanium carbide powder and nickel-based powder deposited on the surface; ferrosilicon is an alloy modifier, which can improve the mechanical properties of basic structural steel, but the overall effect is not good; titanium carbide is enriched at the grain boundary, plays a pinning role, and increases the strength and toughness of the basic structural steel, but due to its small size, it is easy to accumulate into agglomerates, and the use effect is reduced; therefore, titanium carbide is deposited on the surface of ferrosilicon and then added, which effectively improves the strength and toughness of the basic structural steel; and after the grains are refined, it is helpful to carry out carburizing in the subsequent step;
[0030] Electroplating on the surface of basic structural steel can improve the corrosion resistance of basic structural steel on the one hand, and on the other hand, as a transition layer, it is beneficial to improve the uniformity of the carburized layer during the subsequent carburizing step; the modified graphite distributed in the plating layer can serve as the growth core of carbides in the subsequent steps, improve the nucleation rate and help to obtain fine and uniform carbide particles, so that during carburizing, there is no need to first perform low-temperature carburizing to form pre-existing carbide particles, and high-temperature carburizing can be performed directly, thereby improving the carburizing efficiency;
[0031] In order to improve the dispersibility of graphite in the electroplating solution, modifier A is used; the molecular planarity of the pyridine structure in 3-amino-5-fluoropyridine in modifier A helps the coating to be adsorbed on the surface of carbon nanotubes in an orderly manner, and fluorine can play a lubricating role to help obtain a smooth coating; the cationic structure of di(hydroxyethyl)methyldodecylammonium chloride effectively improves the dispersibility of graphite;
[0032] An additive is also added to the electroplating solution. The additive is molybdenum disulfide modified by modifier B. Molybdenum disulfide itself has good lubricity, and its addition helps to improve the performance of the coating. Modifier B includes hyperbranched polyacrylic acid, citric acid ester, and 6-hydroxy-2-pyridinecarboxylic acid. Hyperbranched polyacrylic acid can improve the dispersibility of molybdenum disulfide. Citrate ester and 6-hydroxy-2-pyridinecarboxylic acid have an auxiliary complexing effect, and can also be used as brighteners and leveling agents for electroplating, which help to improve the uniformity of the coating. In summary, the additive helps to form a smooth and uniform coating, and also helps to disperse modified graphite, which has a positive effect on the subsequent carburizing step.
[0033] After carburizing treatment, the surface hardness of structural steel A can be further improved, and its interior can maintain good toughness. However, the conventional carburizing process has the problem that the grains are coarse and affect the performance, and the step of pre-carburizing first takes too long. In the present invention, since modified graphite exists on the surface of structural steel A, high-temperature carburizing can be directly performed, and after high-temperature carburizing, the temperature is lowered to perform low-temperature carburizing, so as to further refine the carbides and reduce the stress in the carburized layer, thereby obtaining a uniform carburized layer. DETAILED DESCRIPTION
[0034] The following is a preferred implementation of the embodiment of the present invention. Obviously, the described embodiment is only a part of the embodiment of the present invention, not all of the embodiments. For ordinary technicians in this technical field, all other embodiments obtained by ordinary technicians in this field without creative work without departing from the principle of the embodiment of the present invention are within the scope of protection of the present invention.
[0035] The following parts are by mass unless otherwise specified;
[0036] Embodiment 1: S1: adding a refining agent to molten iron, refining and slag removal; adding a modifier, modifying treatment; vacuum degassing, continuous casting, rolling in sequence to obtain basic structural steel;
[0037] The modifier comprises the following raw materials, by mass percentage: 55% rare earth ferrosilicon, 25% modified ferrosilicon, 12% silicon-calcium alloy, and 8% trace elements;
[0038] S2: Clean the basic structural steel and electroplate it to obtain structural steel A;
[0039] Specific electroplating process: temperature is 55°C, pH=8, constant current DC current density is 5A / dm 3 , electroplating in the electroplating solution for 12 minutes;
[0040] The electroplating solution includes the following ingredients: 35 g / L nickel sulfate hexahydrate, 10 g / L nickel chloride hexahydrate, 6 g / L zinc sulfate, 5 g / L titanyl sulfate, 55 g / L trisodium citrate, 8 g / L additives, 10 g / L modified graphite, and the rest is water;
[0041] The preparation method of the modified graphite is as follows: (i) taking 12 parts of epoxy silane coupling agent, 6 parts of di(hydroxyethyl)methyl dodecyl ammonium chloride, 3 parts of 3-amino-5-fluoropyridine, and 200 parts of DMSO, heating to 140° C., stirring for 5 hours, and removing the solvent to obtain a modifier A;
[0042] (ii) taking 12 parts of nanographite, 60 parts of ethanol, and 60 parts of water, adding 4 parts of modifier A, stirring at 50° C. for 6 hours, filtering, and drying to obtain modified graphite;
[0043] The preparation method of the additive is as follows: (i) taking 18 parts of hyperbranched polyacrylic acid, 5 parts of citrate, 2 parts of 6-hydroxy-2-pyridinecarboxylic acid, 0.2 parts of stannous isooctanoate, and 0.04 parts of p-toluenesulfonic acid monohydrate, mixing them evenly, heating to 130° C. and stirring for 1 hour, heating to 160° C. and stirring for 5 hours, cooling to 140° C., adding 12 parts of epoxy silane coupling agent, stirring for 5 hours, and removing the solvent to obtain a modifier B;
[0044] (ii) Take 8 parts of molybdenum disulfide, 60 parts of ethanol, and 60 parts of water, add 10 parts of modifier B, and stir at 50° C. for 5 hours to obtain an additive;
[0045] S3: Take structural steel A and perform carburizing: high temperature carburizing: 950℃, carbon potential 1.1, carburizing for 4h, and then cooling in oil at 100℃; low temperature carburizing: 800℃, carbon potential 1.1, carburizing for 3h, and cooling in oil at 100℃; low carbon potential diffusion: 800℃, carbon potential 0.8, diffusion for 1h, quenching and cooling in oil at 100℃; tempering at 180℃ for 3h to obtain high strength and toughness microalloy structural steel.
[0046] Embodiment 2: S1: adding a refining agent to molten iron, refining and slag removal; adding a modifier, modifying treatment; vacuum degassing, continuous casting, rolling in sequence to obtain basic structural steel;
[0047] The modifier comprises the following raw materials, by mass percentage: 55% rare earth ferrosilicon, 25% modified ferrosilicon, 12% silicon-calcium alloy, and 8% trace elements;
[0048] S2: Clean the basic structural steel and electroplate it to obtain structural steel A;
[0049] Specific electroplating process: temperature is 55°C, pH=8, constant current DC current density is 5A / dm 3 , electroplating in the electroplating solution for 12 minutes;
[0050] The electroplating solution includes the following ingredients: 40 g / L nickel sulfate hexahydrate, 5 g / L nickel chloride hexahydrate, 5 g / L zinc sulfate, 10.5 g / L titanyl sulfate, 60 g / L trisodium citrate, 10 g / L additives, 6 g / L modified graphite, and the rest is water;
[0051] The preparation method of the modified graphite is as follows: (i) taking 10 parts of epoxy silane coupling agent, 5 parts of di(hydroxyethyl)methyl dodecyl ammonium chloride, 2 parts of 3-amino-5-fluoropyridine, and 150 parts of DMSO, heating to 130° C., stirring for 6 hours, and removing the solvent to obtain a modifier A;
[0052] (ii) taking 10 parts of nanographite, 40 parts of ethanol, and 40 parts of water, adding 3 parts of modifier A, stirring at 50° C. for 6 hours, filtering, and drying to obtain modified graphite;
[0053] The preparation method of the additive is as follows: (i) taking 15 parts of hyperbranched polyacrylic acid, 4 parts of citrate, 1 part of 6-hydroxy-2-pyridinecarboxylic acid, 0.1 parts of stannous isooctanoate, and 0.04 parts of p-toluenesulfonic acid monohydrate, mixing them evenly, heating to 130° C. and stirring for 1 hour, heating to 160° C. and stirring for 4 hours, cooling to 130° C., adding 10 parts of epoxy silane coupling agent, stirring for 6 hours, and removing the solvent to obtain a modifier B;
[0054] (ii) Take 5 parts of molybdenum disulfide, 40 parts of ethanol, and 40 parts of water, add 8 parts of modifier B, and stir at 50° C. for 5 hours to obtain an additive;
[0055] S3: Take structural steel A and perform carburizing: high temperature carburizing: 900℃, carbon potential 1.1, carburizing for 4h, and then cooling in oil at 100℃; low temperature carburizing: 850℃, carbon potential 1.1, carburizing for 3h, and cooling in oil at 100℃; low carbon potential diffusion: 800℃, carbon potential 0.8, diffusion for 2h, quenching and cooling in oil at 100℃; tempering at 180℃ for 3h to obtain high strength and toughness microalloy structural steel.
[0056] Embodiment 3: S1: adding a refining agent to molten iron, refining and slag removal; adding a modifier, modifying treatment; vacuum degassing, continuous casting, rolling in sequence to obtain basic structural steel;
[0057] The modifier includes the following raw materials, by mass percentage: 55% rare earth ferrosilicon, 25% modified ferrosilicon, 12% silicon-calcium alloy, and 8% trace elements;
[0058] S2: Clean the basic structural steel and electroplate it to obtain structural steel A;
[0059] Specific electroplating process: temperature is 55°C, pH=8, constant current DC current density is 5A / dm 3 , electroplating in the electroplating solution for 12 minutes;
[0060] The electroplating solution includes the following ingredients: 30 g / L nickel sulfate hexahydrate, 15 g / L nickel chloride hexahydrate, 10 g / L zinc sulfate, 3.5 g / L titanyl sulfate, 50 g / L trisodium citrate, 5 g / L additives, 10 g / L modified graphite, and the rest is water;
[0061] The preparation method of the modified graphite is as follows: (i) taking 15 parts of epoxy silane coupling agent, 8 parts of di(hydroxyethyl)methyl dodecyl ammonium chloride, 4 parts of 3-amino-5-fluoropyridine, and 200 parts of DMSO, heating to 140° C., stirring for 6 hours, and removing the solvent to obtain a modifier A;
[0062] (ii) taking 15 parts of nanographite, 60 parts of ethanol and 60 parts of water, adding 5 parts of modifier A, stirring at 50°C for 5 hours, filtering and drying to obtain modified graphite;
[0063] The preparation method of the additive is as follows: (i) taking 20 parts of hyperbranched polyacrylic acid, 6 parts of citrate, 3 parts of 6-hydroxy-2-pyridinecarboxylic acid, 0.2 parts of stannous isooctanoate, and 0.05 parts of p-toluenesulfonic acid monohydrate, mixing them evenly, heating to 130° C. and stirring for 2 hours, heating to 160° C. and stirring for 4 hours, cooling to 140° C., adding 10 parts of epoxy silane coupling agent, stirring for 5 hours, and removing the solvent to obtain a modifier B;
[0064] (ii) Take 10 parts of molybdenum disulfide, 60 parts of ethanol, and 60 parts of water, add 12 parts of modifier B, and stir at 50° C. for 6 hours to obtain an additive;
[0065] S3: Take structural steel A and perform carburizing: high temperature carburizing: 950℃, carbon potential 1.1, carburizing for 4h, and then cooling in oil at 100℃; low temperature carburizing: 800℃, carbon potential 1.1, carburizing for 2h, and cooling in oil at 100℃; low carbon potential diffusion: 800℃, carbon potential 0.8, diffusion for 2h, quenching and cooling in oil at 100℃; tempering at 180℃ for 3h to obtain high strength and toughness microalloy structural steel.
[0066] Comparative Example 1 (nanographite is used instead of modified graphite, and the other method steps are consistent with Example 1): S1: adding a refining agent to molten iron, refining and slag removal; adding a modifier, and performing a modification treatment; vacuum degassing, continuous casting, and rolling are performed in sequence to obtain basic structural steel;
[0067] The modifier comprises the following raw materials, by mass percentage: 55% rare earth ferrosilicon, 25% modified ferrosilicon, 12% silicon-calcium alloy, and 8% trace elements;
[0068] S2: Clean the basic structural steel and electroplate it to obtain structural steel A;
[0069] Specific electroplating process: temperature is 55°C, pH=8, constant current DC current density is 5A / dm 3 , electroplating in the electroplating solution for 12 minutes;
[0070] The electroplating solution includes the following ingredients: 35 g / L nickel sulfate hexahydrate, 10 g / L nickel chloride hexahydrate, 6 g / L zinc sulfate, 5 g / L titanyl sulfate, 55 g / L trisodium citrate, 8 g / L additives, 10 g / L nanographite, and the rest is water;
[0071] The preparation method of the additive is as follows: (i) taking 18 parts of hyperbranched polyacrylic acid, 5 parts of citrate, 2 parts of 6-hydroxy-2-pyridinecarboxylic acid, 0.2 parts of stannous isooctanoate, and 0.04 parts of p-toluenesulfonic acid monohydrate, mixing them evenly, heating to 130° C. and stirring for 1 hour, heating to 160° C. and stirring for 5 hours, cooling to 140° C., adding 12 parts of epoxy silane coupling agent, stirring for 5 hours, and removing the solvent to obtain a modifier B;
[0072] (ii) Take 8 parts of molybdenum disulfide, 60 parts of ethanol, and 60 parts of water, add 10 parts of modifier B, and stir at 50° C. for 5 hours to obtain an additive;
[0073] S3: Take structural steel A and perform carburizing: high temperature carburizing: 950℃, carbon potential 1.1, carburizing for 4h, and then cooling in oil at 100℃; low temperature carburizing: 800℃, carbon potential 1.1, carburizing for 3h, and cooling in oil at 100℃; low carbon potential diffusion: 800℃, carbon potential 0.8, diffusion for 1h, quenching and cooling in oil at 100℃; tempering at 180℃ for 3h to obtain high strength and toughness microalloy structural steel.
[0074] Comparative Example 2 (the preparation method of the additive is changed, and the other method steps are consistent with Example 1): S1: adding a refining agent to molten iron, refining and slag removal; adding a modifier, and performing a modification treatment; vacuum degassing, continuous casting, and rolling are performed in sequence to obtain basic structural steel;
[0075] The modifier includes the following raw materials, by mass percentage: 55% rare earth ferrosilicon, 25% modified ferrosilicon, 12% silicon-calcium alloy, and 8% trace elements;
[0076] S2: Clean the basic structural steel and electroplate it to obtain structural steel A;
[0077] Specific electroplating process: temperature is 55°C, pH=8, constant current DC current density is 5A / dm 3 , electroplating in the electroplating solution for 12 minutes;
[0078] The electroplating solution includes the following ingredients: 35 g / L nickel sulfate hexahydrate, 10 g / L nickel chloride hexahydrate, 6 g / L zinc sulfate, 5 g / L titanyl sulfate, 55 g / L trisodium citrate, 8 g / L additives, 10 g / L modified graphite, and the rest is water;
[0079] The preparation method of the modified graphite is as follows: (i) taking 12 parts of epoxy silane coupling agent, 6 parts of di(hydroxyethyl)methyl dodecyl ammonium chloride, 3 parts of 3-amino-5-fluoropyridine, and 200 parts of DMSO, heating to 140° C., stirring for 5 hours, and removing the solvent to obtain a modifier A;
[0080] (ii) taking 12 parts of nanographite, 60 parts of ethanol, and 60 parts of water, adding 4 parts of modifier A, stirring at 50° C. for 6 hours, filtering, and drying to obtain modified graphite;
[0081] The preparation method of the additive is as follows: (i) taking 2 parts of 6-hydroxy-2-pyridinecarboxylic acid and 2 parts of epoxy silane coupling agent, stirring for 5 hours, and removing the solvent to obtain a modifier B;
[0082] (ii) Take 8 parts of molybdenum disulfide, 60 parts of ethanol, and 60 parts of water, add 10 parts of modifier B, and stir at 50° C. for 5 hours to obtain an additive;
[0083] S3: Take structural steel A and perform carburizing: high temperature carburizing: 950℃, carbon potential 1.1, carburizing for 4h, and then cooling in oil at 100℃; low temperature carburizing: 800℃, carbon potential 1.1, carburizing for 3h, and cooling in oil at 100℃; low carbon potential diffusion: 800℃, carbon potential 0.8, diffusion for 1h, quenching and cooling in oil at 100℃; tempering at 180℃ for 3h to obtain high strength and toughness microalloy structural steel.
[0084] Comparative Example 3 (modifier A is used to replace modified graphite, and the remaining steps are consistent with those of Example 1): S1: adding a refining agent to molten iron, refining and slagging; adding a modifier, and performing a modification treatment; vacuum degassing, continuous casting, and rolling are performed in sequence to obtain basic structural steel;
[0085] The modifier comprises the following raw materials, by mass percentage: 55% rare earth ferrosilicon, 25% modified ferrosilicon, 12% silicon-calcium alloy, and 8% trace elements;
[0086] S2: Clean the basic structural steel and electroplate it to obtain structural steel A;
[0087] Specific electroplating process: temperature is 55°C, pH=8, constant current DC current density is 5A / dm 3 , electroplating in the electroplating solution for 12 minutes;
[0088] The electroplating solution includes the following ingredients: 35 g / L nickel sulfate hexahydrate, 10 g / L nickel chloride hexahydrate, 6 g / L zinc sulfate, 5 g / L titanyl sulfate, 55 g / L trisodium citrate, 8 g / L additives, 10 g / L modifier A, and the rest is water;
[0089] The preparation method of the modifier A is as follows: 12 parts of epoxy silane coupling agent, 6 parts of di(hydroxyethyl)methyl dodecyl ammonium chloride, 3 parts of 3-amino-5-fluoropyridine, and 200 parts of DMSO are taken, heated to 140° C., stirred for 5 hours, and the solvent is removed to obtain the modifier A;
[0090] The preparation method of the additive is as follows: (i) taking 18 parts of hyperbranched polyacrylic acid, 5 parts of citrate, 2 parts of 6-hydroxy-2-pyridinecarboxylic acid, 0.2 parts of stannous isooctanoate, and 0.04 parts of p-toluenesulfonic acid monohydrate, mixing them evenly, heating to 130° C. and stirring for 1 hour, heating to 160° C. and stirring for 5 hours, cooling to 140° C., adding 12 parts of epoxy silane coupling agent, stirring for 5 hours, and removing the solvent to obtain a modifier B;
[0091] (ii) Take 8 parts of molybdenum disulfide, 60 parts of ethanol, and 60 parts of water, add 10 parts of modifier B, and stir at 50° C. for 5 hours to obtain an additive;
[0092] S3: Take structural steel A and perform carburizing: high temperature carburizing: 950℃, carbon potential 1.1, carburizing for 4h, and then cooling in oil at 100℃; low temperature carburizing: 800℃, carbon potential 1.1, carburizing for 3h, and cooling in oil at 100℃; low carbon potential diffusion: 800℃, carbon potential 0.8, diffusion for 1h, quenching and cooling in oil at 100℃; tempering at 180℃ for 3h to obtain high strength and toughness microalloy structural steel.
[0093] Comparative Example 4 (the raw material of the modifier is changed, and the other method steps are consistent with Example 1): S1: adding a refining agent to molten iron, refining and slag removal; adding a modifier, and performing a modification treatment; vacuum degassing, continuous casting, and rolling are performed in sequence to obtain basic structural steel;
[0094] The modifier comprises the following raw materials, by mass percentage: 40% rare earth ferrosilicon, 20% ferrosilicon, 20% titanium carbide, 12% silicon-calcium alloy, and 8% trace elements;
[0095] S2: Clean the basic structural steel and electroplate it to obtain structural steel A;
[0096] Specific electroplating process: temperature is 55°C, pH=8, constant current DC current density is 5A / dm 3 , electroplating in the electroplating solution for 12 minutes;
[0097] The electroplating solution includes the following ingredients: 35 g / L nickel sulfate hexahydrate, 10 g / L nickel chloride hexahydrate, 6 g / L zinc sulfate, 5 g / L titanyl sulfate, 55 g / L trisodium citrate, 8 g / L additives, 10 g / L modified graphite, and the rest is water;
[0098] The preparation method of the modified graphite is as follows: (i) taking 12 parts of epoxy silane coupling agent, 6 parts of di(hydroxyethyl)methyl dodecyl ammonium chloride, 3 parts of 3-amino-5-fluoropyridine, and 200 parts of DMSO, heating to 140° C., stirring for 5 hours, and removing the solvent to obtain a modifier A;
[0099] (ii) taking 12 parts of nanographite, 60 parts of ethanol, and 60 parts of water, adding 4 parts of modifier A, stirring at 50° C. for 6 hours, filtering, and drying to obtain modified graphite;
[0100] The preparation method of the additive is as follows: (i) taking 18 parts of hyperbranched polyacrylic acid, 5 parts of citrate, 2 parts of 6-hydroxy-2-pyridinecarboxylic acid, 0.2 parts of stannous isooctanoate, and 0.04 parts of p-toluenesulfonic acid monohydrate, mixing them evenly, heating to 130° C. and stirring for 1 hour, heating to 160° C. and stirring for 5 hours, cooling to 140° C., adding 12 parts of epoxy silane coupling agent, stirring for 5 hours, and removing the solvent to obtain a modifier B;
[0101] (ii) Take 8 parts of molybdenum disulfide, 60 parts of ethanol, and 60 parts of water, add 10 parts of modifier B, and stir at 50° C. for 5 hours to obtain an additive;
[0102] S3: Take structural steel A and perform carburizing: high temperature carburizing: 950℃, carbon potential 1.1, carburizing for 4h, and then cooling in oil at 100℃; low temperature carburizing: 800℃, carbon potential 1.1, carburizing for 3h, and cooling in oil at 100℃; low carbon potential diffusion: 800℃, carbon potential 0.8, diffusion for 1h, quenching and cooling in oil at 100℃; tempering at 180℃ for 3h to obtain high strength and toughness microalloy structural steel.
[0103] In the above embodiments, the test methods used are conventional methods unless otherwise specified; the raw materials used are commercially available unless otherwise specified, and the sources of the raw materials are as follows: nickel sulfate hexahydrate (CAS: 10101-97-0); nickel chloride hexahydrate (W00416, Wuhan Jiye Sheng); zinc sulfate (S22124, Shanghai Yuanye); titanyl sulfate (S41632, Shanghai Yuanye); trisodium citrate (S67462, Shanghai Yuanye); epoxy silane coupling agent (KH560, S15029, Shanghai Yuanye); di(hydroxyethyl)methyl dodecyl ammonium chloride (Y17642, Shanghai Yuanye); 3-amino-5-fluoropyridine (CAS: 210169-05-4); DMSO (CAS: 67-68-5); nanographite (40nm, Kramar); ethanol (C AS: 64-17-5); hyperbranched polyacrylic acid (H20-star-PAA, Xi'an Ruixi Biotechnology Co., Ltd.); citrate ester (B20912, Shanghai Yuanye); rare earth ferrosilicon (rare earth 17% ~ 37%, Si35% ~ 46%, Mn5% ~ 8%, Ca5% ~ 8%, Ti6%, the rest is iron; Anyang Jinsheng Metallurgical Materials Co., Ltd.); ferrosilicon (FeSi75-C, Beijing Jingang); silicon calcium alloy (Ca content 30%); 6-hydroxy-2-pyridinecarboxylic acid (CAS: 19621-92-2); stannous isooctanoate (S3252, Sigma-Aldrich); p-toluenesulfonic acid monohydrate (CAS: 6192-52-5); molybdenum disulfide (S30491, Shanghai Yuanye); titanium carbide powder (TIC1235, Yumu New Materials Co., Ltd.).
[0104] Experiment: Take the high-strength and toughness microalloy structural steel prepared in Examples 1 to 3 and Comparative Examples 1 to 4; (1) Use a 430SVD Vickers hardness tester to measure the Vickers hardness at 1 cm, with a load of 200 g; (2) Use a JB-30B drop hammer impact tester to perform an impact test, with an impact specimen size of 10×10×55 mm; see the table below for specific data;
[0105]
[0106] Conclusion: In comparative example 1, nanographite is used instead of modified graphite. Due to the poor dispersibility of nanographite in the electroplating solution, the nanographite is unevenly distributed in the coating, which affects carburizing and significantly reduces the performance; in comparative example 2, the additive preparation method is changed. Due to the change in the coating state, the performance is not as good as that of the embodiment; in comparative example 3, modifier A is used instead of modified graphite, that is, nanographite is not introduced, which has a greater impact on the carburizing process and significantly reduces the performance; in comparative example 4, the raw material of the modifier is changed, and the performance is reduced, from which the importance of a suitable modifier can be seen; in summary, the microalloy structural steel prepared by the present invention has the characteristics of high strength and high toughness.
[0107] Finally, it should be noted that the above is only a preferred embodiment of the present invention, but the protection scope of this application is not limited thereto. Any changes or substitutions that can be easily thought of by any technician familiar with the technical field within the spirit and principle of the present invention and within the technical scope disclosed in this application should be included in the protection scope of this application; in the absence of conflict, the embodiments of this application and the features in the embodiments can be combined with each other. Therefore, the protection scope of this application shall be based on the protection scope of the claims.
Claims
1. A method for preparing high-strength and high-toughness microalloy structural steel, characterized in that: The following steps are involved: S1: adding refining agent to molten iron, refining and slag removal; adding modifier, modification treatment; Vacuum degassing, continuous casting and rolling are carried out in sequence to obtain basic structural steel; S2: The basic structural steel is cleaned and electroplated to obtain structural steel A with modified graphite deposited on the surface; S3: Take structural steel A and perform high temperature carburizing, low temperature carburizing, diffusion, quenching cooling, and tempering in sequence to obtain high strength and toughness microalloy structural steel.
2. The method for preparing a high-strength and toughness microalloy structural steel according to claim 1, characterized in that: The molten iron includes the following components in percentage by mass: C: 0.7-0.85%, Si: 0.15-0.35%, Mn: 0.70-0.90%, P: ≤0.025%, S: ≤0.025%, Cr: 0.16-0.25%, V: 0.068-0.08%, Cu: ≤0.001%, Ni: ≤0.001%, Ti: ≤0.001%, and the rest are Fe and unavoidable impurities.
3. The method for preparing a high-strength and toughness microalloy structural steel according to claim 1, characterized in that: In step S2, the specific process of electroplating is: controlling the temperature to 50-60°C, pH to 7-8, and the current density to 4-6A / dm 3 , electroplating in the electroplating solution for 10 to 15 minutes; The electroplating solution includes the following raw materials: 30-40 g / L nickel sulfate hexahydrate, 5-15 g / L nickel chloride hexahydrate, 5-10 g / L zinc sulfate, 3.5-10.5 g / L titanyl sulfate, 50-60 g / L trisodium citrate, 5-10 g / L additives, 5-10 g / L modified graphite, and the rest is water.
4. The method for preparing a high-strength and toughness microalloy structural steel according to claim 3, characterized in that: The preparation of the modified graphite comprises the following steps: Step 1: taking an epoxy silane coupling agent, di(hydroxyethyl)methyl dodecyl ammonium chloride, 3-amino-5-fluoropyridine, and DMSO, heating to 130-140° C., stirring for 4-6 hours, and removing the solvent to obtain a modifier A; Step 2: Take nanographite, ethanol, and water, add modifier A, stir at 40-50° C. for 5-6 hours, filter, and dry to obtain modified graphite; The modifier A comprises the following raw materials, calculated by weight: 10 to 15 parts of epoxy silane coupling agent, 5 to 8 parts of di(hydroxyethyl)methyl dodecyl ammonium chloride, 2 to 4 parts of 3-amino-5-fluoropyridine, and 150 to 200 parts of DMSO; The modified graphite comprises the following raw materials, calculated by weight: 10 to 15 parts of nanographite, 40 to 60 parts of ethanol, 40 to 60 parts of water, and 3 to 5 parts of modifier A.
5. The method for preparing a high-strength and toughness microalloy structural steel according to claim 3, characterized in that: The preparation of the additive comprises the following steps: Step 1: taking portions of hyperbranched polyacrylic acid, citrate, 6-hydroxy-2-pyridinecarboxylic acid, stannous isooctanoate, and p-toluenesulfonic acid monohydrate, mixing them uniformly, heating to 130-140° C. and stirring for 1-2 hours, heating to 150-160° C. and stirring for 4-6 hours, cooling to 130-140° C., adding an epoxy silane coupling agent, stirring for 4-6 hours, and removing the solvent to obtain a modifier B; Step 2: Take molybdenum disulfide, ethanol, and water, add modifier B, and stir at 40-50° C. for 5-6 hours to obtain an additive; The modifier B comprises the following raw materials, calculated by mass: 15 to 20 parts of hyperbranched polyacrylic acid, 4 to 6 parts of citrate, 1 to 3 parts of 6-hydroxy-2-pyridinecarboxylic acid, 0.1 to 0.2 parts of stannous isooctanoate, 0.04 to 0.05 parts of p-toluenesulfonic acid monohydrate, and 10 to 15 parts of epoxy silane coupling agent; The additive comprises the following raw materials, calculated by weight: 5 to 10 parts of molybdenum disulfide, 40 to 60 parts of ethanol, 40 to 60 parts of water, and 8 to 12 parts of modifier B.
6. The method for preparing a high-strength and toughness microalloy structural steel according to claim 1, characterized in that: In step S2, the specific process of high-temperature carburizing is as follows: the temperature is 900-950°C, the carbon potential is 1.1, and the time is 3-4h; the specific process of low-temperature carburizing is as follows: the temperature is 800-850°C, the carbon potential is 1.1, and the time is 2-3h; the specific process of diffusion is as follows: the temperature is 800-850°C, the carbon potential is 0.8, and the time is 1-2h.
7. The method for preparing a high-strength and toughness microalloy structural steel according to claim 1, characterized in that: The adding amount of the refining agent and the modifying agent is 1-2% of the mass of the molten iron respectively.
8. The method for preparing a high-strength and toughness microalloy structural steel according to claim 7, characterized in that: The refining agent includes the following raw materials, by mass percentage: 80-90% CaO, 10-20% Al2O3; the modifier includes the following raw materials, by mass percentage: 50-60% rare earth ferrosilicon, 20-30% modified ferrosilicon, 10-20% silicon-calcium alloy, 5-10% trace elements; the trace elements include the following raw materials, by mass percentage: 40% Zr, 25% Cu, 15% Sb, 15% Bi and 5% B.
9. The method for preparing a high-strength and toughness microalloy structural steel according to claim 8, characterized in that: The preparation of the modified ferrosilicon comprises the following steps: Titanium carbide powder and nickel-based powder are mixed in a mass ratio of (1-2):1 to obtain a mixture; the mixture is deposited on the surface of ferrosilicon by plasma transfer arc welding to obtain modified ferrosilicon.
10. High-strength and toughness microalloyed structural steel prepared according to the method for preparing high-strength and toughness microalloyed structural steel according to any one of claims 1 to 9.
Citation Information
Patent Citations
Surface alloying strengthening method
CN103184457A
High-strength impact-resistance type steel used for shelf beam and welding technology thereof
CN104762558A
Preparation method of nickel-modified graphene abrasion-resistant composite coating
CN107630244A
Bright black nickel plating electroplate solution and preparation method and application thereof
CN111270275A
Machining method of wear-resistant gear for miniature speed reducer
CN114351081A
Cited By
Low-carbon aluminum killed steel and manufacturing process thereof
CN119571187A