Current collector coating assembly and coating method

By setting grooves on the evaporation cooling drum and applying an epoxy resin coating doped with graphene oxide, the problem of deposition and peeling of plating materials in drum-type coating equipment is solved, and product quality and production efficiency are improved .

CN119082672APending Publication Date: 2024-12-06JIANGYIN NANOPORE INNOVATIVE MATERIALS TECH LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411196077.0
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

When using drum-mounted vacuum coating equipment, material deposition and coating peeling problems in areas where the vapor deposition cooling drum is not covered by the film lead to product quality and efficiency, and existing solutions increase cutting waste and waste.

Method used

The unfilled area on the evaporation cooling drum is provided with grooves, and the inner wall of the groove is coated with graphene oxide-doped epoxy resin coating with binding force for bearing and fixing plating materials to reduce the Plating material deposits and sheds.

Benefits of technology

It effectively reduces the poor cooling effect and edge whitening or curling problems caused by deposition of the plating materials, improves the quality and efficiency of coating products, and reduces cutting waste and waste.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082672A_ABST
    Figure CN119082672A_ABST
Patent Text Reader

Abstract

The current collector coating assembly comprises an evaporation source, a baffle above the evaporation source and an evaporation cooling drum above the baffle, the middle of the evaporation cooling drum is a thin film covering area, a groove is formed in the area, not covered by a thin film, of the evaporation cooling drum, and the inner wall of the groove is coated with a coating having binding force with a coating material. According to the invention, drum-attached film coating is adopted, the groove is additionally arranged, and the coating with binding force with the plating material is coated in the groove, so that the plating material which is deposited without being covered by the film is received and is firmly attached to the groove, and the product quality problem caused by material falling due to the fact that the plating material is deposited on the drum in the evaporation process is reduced.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The present invention relates to the field of current collectors, and in particular to a current collector coating component and a coating method. Background Art

[0002] The current collector is an important component of the secondary battery. At present, the composite current collector with a metal-polymer material-metal structure is used to replace the traditional copper foil or aluminum foil current collector, which can effectively reduce the weight of the battery current collector and improve the battery safety and energy density. With the development of vacuum coating, the production process of flexible conductive films has gradually replaced traditional electroplating, coating and chemical treatment methods by vacuum coating, which reduces pollution and has the advantages of strong coating bonding and uniform film layer.

[0003] There are currently two types of vacuum coating equipment on the market, one is the drum-type coating equipment, and the other is the suspension coating equipment. Among them, the drum-type coating equipment is equipped with an evaporation cooling drum, which can achieve double-sided one-time film formation, which can greatly improve production efficiency. However, when using the drum-type coating, the cooling drum is set above the evaporation area, and the length of the drum is greater than the width of the film. If the opening of the baffle set on the evaporation source is the same width as the film surface, it will cause the material to diffuse to the drum that is not covered by the film. The material is deposited on the drum, affecting the cooling effect of the drum, and as the coating thickens, there will be a risk of falling off, affecting the product quality. Therefore, in order to avoid this situation, the evaporation baffle opening is generally set smaller than the width of the film when using the drum-type coating, blocking the edge of the film to prevent the material from being deposited on the evaporation cooling drum. However, there are still some problems with this. The size of the baffle will also cause the edge of the film surface to be left blank or the film to form a drum edge warping phenomenon, thereby increasing the process of cutting waste materials and wasting part of the base film, which ultimately affects product quality and product yield. Summary of the invention

[0004] The object of the present invention is to provide a current collector coating assembly and a coating method in view of the above problems.

[0005] To achieve the above purpose, the technical solution provided by the present invention is:

[0006] A current collector coating assembly comprises an evaporation source, a baffle above the evaporation source and an evaporation cooling drum above the baffle, wherein the middle portion of the evaporation cooling drum is a film-covered area, and an area on the evaporation cooling drum that is not covered by the film is provided with a groove, and the inner wall of the groove is coated with a coating having bonding force with a coating material.

[0007] To optimize the above technical solutions, the specific measures taken also include:

[0008] The grooves are arranged on the left and right sides of the film covering area on the evaporation cooling drum, and the grooves are adjacent to the film covering area of ​​the cooling drum.

[0009] Furthermore, the groove has a width of 2-10 cm and a depth of 0.5-2 cm.

[0010] The coating is an epoxy resin coating doped with graphene oxide.

[0011] Furthermore, the epoxy resin coating doped with graphene oxide is composed of epoxy resin, graphene oxide, a curing agent and an auxiliary agent, and the mass ratio thereof is 100:10-40:50-60:15-24; the auxiliary agent includes at least one of a coupling agent, an antioxidant and a plasticizer.

[0012] Preferably, the epoxy resin is selected from one or more of acrylic epoxy resin, glycerol epoxy resin, bisphenol A epoxy resin E51, and alicyclic epoxy resin; the curing agent is selected from one or more of triethylenetetramine, diaminodiphenylmethane, and isophoronediamine; the graphene oxide has a thickness of 0.6 to 1.2 nm, a number of layers of 1 to 5 layers, a size of 50 to 300 μm, and an oxygen content of 30% to 40%.

[0013] Preferably, the coupling agent is selected from one or more of silane coupling agent, titanate coupling agent, aluminate coupling agent, and bimetallic coupling agent; the antioxidant is selected from one or more of antioxidant DNP, antioxidant 264, and phenyl salicylate; the plasticizer is selected from one or more of DOS plasticizer, ESO plasticizer, and stearic acid.

[0014] The present invention also provides a current collector coating method using drum-type coating, wherein a groove is added to the area on the evaporation cooling drum that is not covered by the film, and the groove is used to receive the coating material deposited on the evaporation cooling drum because it is not covered by the film; a coating having bonding force with the coating material is coated on the inner wall of the groove, and the coating is used to make the coating material firmly adhere to the groove.

[0015] Furthermore, the coating is obtained by coating with an epoxy resin coating doped with graphene oxide and then curing the coating; wherein the preparation steps of the epoxy resin coating doped with graphene oxide are as follows:

[0016] adding graphene oxide to epoxy resin and stirring to obtain a mixed material;

[0017] A curing agent and an auxiliary agent are added to the mixed material, and the mixture is stirred to obtain an epoxy resin coating doped with graphene oxide.

[0018] Furthermore, during the coating process, the coating is replaced after the aluminum layer in the groove accumulates to a specified thickness, or it is determined whether the coating needs to be replaced based on the observation of dealumination during the evaporation process; when replacing the coating, the temperature of the evaporation cooling drum is increased to make the coating fall off, the fallen coating in the groove is cleaned, the coating is re-applied in the groove, and after curing, subsequent coating is carried out.

[0019] Compared with the prior art, the present invention has the following beneficial effects:

[0020] The present invention provides a current collector coating component and a coating method, which use drum-type coating to reduce product quality problems caused by material shedding due to deposition of coating materials on the drum during evaporation by adding grooves and coatings.

[0021] The present invention adds a groove in the area not covered by the film on the evaporation cooling drum, and the groove part can receive the plated material deposited on the evaporation cooling drum, thereby reducing the problem of poor cooling effect caused by the plated material being deposited on the drum or the problem of blank space and warping of the film surface caused by the retaining edge.

[0022] The present invention coats the inner wall of the groove with a coating having bonding force with the plating material, which can increase the bonding force between the plating material and the coating, and reduce the product quality problem caused by the material falling off due to the deposition of the plating material on the drum during the evaporation process. During the evaporation process, the evaporation cooling drum is in a low temperature state. Due to the introduction of the coating, the bonding force between the plating material and the groove part is greater, and the plating material is firmly attached to the groove, so that the plating material is not easy to fall off.

[0023] The present invention has been verified through experiments that coating the inner walls of the grooves added on both sides of the film covering area on the evaporation cooling drum with a coating having bonding strength with the plated material, such as an epoxy resin coating doped with graphene oxide, has a better effect.

[0024] After several times of coating, the coating is replaced after the aluminum layer in the groove accumulates to a certain thickness, or the need to replace the coating can be determined by observing the dealuminization phenomenon during the evaporation process; when replacing the coating, the temperature of the evaporation cooling drum is increased. Under high temperature conditions, the epoxy resin coating is easy to fall off, which is convenient for cleaning the plating material residue in the groove. This method is simple, easy to implement and easy to operate. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 : A schematic structural diagram of the current collector coating assembly of the present invention.

[0026] In the figure: 1-evaporation source, 2-baffle, 3-evaporation cooling drum, 4-film covering area, 5-groove. DETAILED DESCRIPTION

[0027] The above contents of the present invention are further described in detail below in the form of embodiments, but this should not be understood as the scope of the above subject matter of the present invention being limited to the following embodiments, and all technologies realized based on the above contents of the present invention belong to the scope of the present invention.

[0028] The experimental methods used in the following examples are all conventional methods unless otherwise specified, and the reagents, methods and equipment used are all conventional reagents, methods and equipment in the technical field unless otherwise specified.

[0029] like Figure 1 As shown, the present invention provides a current collector coating assembly, including an evaporation source 1, a baffle 2 above the evaporation source and an evaporation cooling drum 3 above the baffle 2, the middle portion of the evaporation cooling drum 3 is a film covering area 4, and a groove 5 is provided in the area on the evaporation cooling drum 3 that is not covered by the film, and the inner wall of the groove 5 is coated with a coating that has bonding force with the coating material.

[0030] The groove width is 2-10 cm and the depth is 0.5-2 cm. Preferably, the groove width is 3-6 cm and the depth is 0.5-1 cm.

[0031] The present invention also provides a current collector coating method, which uses drum-type coating and adds a groove 5 in the area of ​​the evaporation cooling drum 3 that is not covered by the film. The groove 5 is used to receive the coating material deposited on the evaporation cooling drum because it is not covered by the film; a coating that has bonding force with the coating material is coated on the inner wall of the groove 5, and the coating is used to make the coating material firmly adhere to the groove 5.

[0032] The present invention preferably uses an epoxy resin coating doped with graphene oxide. The preparation steps of the epoxy resin coating doped with graphene oxide are as follows:

[0033] adding graphene oxide to epoxy resin and stirring to obtain a mixed material;

[0034] A curing agent and an auxiliary agent are added to the mixed material, and the mixture is stirred to obtain an epoxy resin coating doped with graphene oxide.

[0035] After one round of coating is completed, the coating is removed by increasing the temperature of the evaporation cooling drum. The removed coating in the groove is cleaned, and the coating is re-applied in the groove and cured before the next round of coating is carried out.

[0036] Preferably, the coating is cured by heating.

[0037] Example 1

[0038] In this embodiment, a composite aluminum current collector is prepared using an evaporation cooling drum provided with a groove and the inner wall of the groove is coated with an epoxy resin coating doped with graphene oxide. The specific steps are as follows:

[0039] (1) On a cylindrical evaporation cooling drum, according to the width of the film produced by the equipment, a groove is opened in the area not covered by the film at the edge of the film, with a width of 5 cm and a depth of 1 cm;

[0040] (2) Preparation of epoxy resin coating doped with graphene oxide: 100 g of bisphenol A epoxy resin E51 (solid content 50%) was taken, 20 g of graphene oxide was added, and mechanical stirring was performed for 5 min for dispersion at a speed of 500 r / min to obtain a mixed slurry A, wherein the graphene oxide had a thickness of 0.8 to 0.9 nm, a number of layers of 4 layers, a size of about 200 μm, and an oxygen content of about 35%. Then 3 g of silane coupling agent KH550 and 2 g of antioxidant DNP were taken and added to the mixed slurry A. The mixture was dispersed by mechanical stirring for 5 minutes at a speed of 500 r / min to obtain a mixed slurry B; 50 g of isophorone diamine (IPDA) and 10 g of stearic acid were then added to the mixed slurry B, and the mixture was dispersed by mechanical stirring for 5 minutes at a speed of 500 r / min to obtain an epoxy resin coating doped with graphene oxide; finally, the prepared epoxy resin coating doped with graphene oxide was evenly coated on the inner wall of the groove of the evaporation cooling drum, and heated and cured to obtain an epoxy resin coating with a coating thickness of 300 μm.

[0041] (3) The above-mentioned evaporation cooling drum with grooves and coating is applied to the winding system of the vacuum evaporation chamber to evaporate metal aluminum on flexible base films such as PET / PPPI to prepare a composite aluminum current collector, wherein the coating speed is 240m / min, the wire feeding speed is 480m / min, and the aluminum film thickness is 1μm.

[0042] During the coating process, the aluminum accumulation in the groove area was observed. Compared with Comparative Example 1 (see below), it was found that the dealumination phenomenon was significantly reduced, and there was no blank space or curling or warping defects on the membrane surface of the composite current collector product.

[0043] Example 2

[0044] The preparation method is exactly the same as that of Example 1, except that the amount of graphene oxide used is 30 g. The results show that during the coating process, the dealumination phenomenon after aluminum accumulation in the groove area is less than that in Example 1, and the composite current collector product has no blank space on the film surface and no curling or warping defects.

[0045] Comparative Example 1

[0046] The interior of the groove of the evaporation cooling drum used in this comparative example is not coated with an epoxy resin coating doped with graphene oxide, and the rest of the preparation method is the same as that of Example 1.

[0047] The results showed that due to the grooves in the evaporation cooling drum, the prepared composite current collector product had no blank space and no curling or warping defects on the membrane surface; however, during the coating process, the dealumination phenomenon was obvious after aluminum accumulation in the groove area, and some aluminum chips were observed to fall off and splash onto the product surface, resulting in an increase in the number of bumps and pinholes on the product membrane surface.

[0048] Comparative Example 2

[0049] In this comparative example, a composite aluminum current collector is prepared using an evaporation cooling drum without grooves, a baffle covers the edge of the membrane surface by about 1 cm, and there is no epoxy resin coating; the rest of the preparation method is the same as that in Example 1.

[0050] The results showed that during the coating process, blank spaces and partial curling and warping defects occurred on the surface of the composite current collector product; aluminum chips fell off and splashed onto the surface of the product, resulting in multiple bumps and pinholes on the surface of the product film.

[0051] Table 1 Measurement results of embodiments and comparative examples

[0052]

[0053] The parameters in Table 1 were determined as follows:

[0054] Number of bumps: Counting by CCD. Place the sample on a rewinder equipped with CCD detection equipment, rewind the produced sample, and count the bumps on the sample by CCD.

[0055] Number of pinholes: measured by a flaw detector. Cut a 1×1m sample and place it on the flaw detector's detection surface. Ensure that it is opaque all around. Turn off the indoor lights and observe from a height of about 0.5m. Count the visible pinholes on the sample.

[0056] Edge margin: Use a steel ruler to measure the margin of the composite current collector product membrane surface;

[0057] Edge warping height: Cut a 1×1m sample, place the sample on a horizontal table, and use a steel ruler to measure the distance the product edge is raised relative to the table.

[0058] The above description is only a preferred embodiment of the present invention and does not limit the present invention in any form. Any technician familiar with the profession, without departing from the scope of the technical solution of the present invention, according to the technical essence of the present invention, any simple modification, equivalent replacement and improvement made to the above embodiment still falls within the protection scope of the technical solution of the present invention.

Claims

1. A current collector coating assembly, comprising an evaporation source, a baffle above the evaporation source, and an evaporation cooling drum above the baffle, characterized in that: The middle part of the evaporation cooling drum is a film-covered area, and a groove is arranged in the area of ​​the evaporation cooling drum not covered by the film. The inner wall of the groove is coated with a coating having bonding force with the plating material.

2. The current collector coating assembly according to claim 1, characterized in that: The grooves are arranged on the left and right sides of the film covering area on the evaporation cooling drum, and the grooves are adjacent to the film covering area of ​​the cooling drum.

3. The current collector coating assembly according to claim 1, characterized in that: The groove has a width of 2-10 cm and a depth of 0.5-2 cm.

4. The current collector coating assembly according to claim 1, characterized in that: The coating is an epoxy resin coating doped with graphene oxide.

5. The current collector coating assembly according to claim 4, characterized in that: The epoxy resin coating doped with graphene oxide is composed of epoxy resin, graphene oxide, curing agent and auxiliary agent, and the weight ratio thereof is 100:10-40:50-60:15-24; the auxiliary agent includes at least one of a coupling agent, an antioxidant and a plasticizer.

6. The current collector coating assembly according to claim 5, characterized in that: The epoxy resin is selected from one or more of acrylic epoxy resin, glycerol epoxy resin, bisphenol A epoxy resin E51, and alicyclic epoxy resin; the curing agent is selected from one or more of triethylenetetramine, diaminodiphenylmethane, and isophoronediamine; the graphene oxide has a thickness of 0.6 to 1.2 nm, a number of layers of 1 to 5 layers, a size of 50 to 300 μm, and an oxygen content of 30% to 40%.

7. The current collector coating assembly according to claim 5, characterized in that: The coupling agent is selected from one or more of silane coupling agent, titanate coupling agent, aluminate coupling agent, and bimetallic coupling agent; the antioxidant is selected from one or more of antioxidant DNP, antioxidant 264, and phenyl salicylate; the plasticizer is selected from one or more of DOS plasticizer, ESO plasticizer, and stearic acid.

8. A current collector coating method, characterized in that: Using drum-type coating, a groove is added to the area on the evaporation and cooling drum that is not covered by the film. The groove is used to receive the plating material deposited on the evaporation and cooling drum because it is not covered by the film; a coating that has bonding strength with the plating material is coated on the inner wall of the groove, and the coating is used to make the plating material firmly adhere to the groove.

9. The current collector coating method according to claim 8, characterized in that: The coating is obtained by coating with an epoxy resin coating doped with graphene oxide and then curing the coating; wherein the preparation steps of the epoxy resin coating doped with graphene oxide are as follows: adding graphene oxide to epoxy resin and stirring to obtain a mixed material; A curing agent and an auxiliary agent are added to the mixed material, and the mixture is stirred to obtain an epoxy resin coating doped with graphene oxide.

10. The current collector coating method according to claim 8, characterized in that: During the coating process, the coating is replaced when the aluminum layer in the groove accumulates to a specified thickness, or the coating needs to be replaced based on the dealuminization phenomenon observed during the evaporation process; When replacing the coating, the temperature of the evaporation cooling drum is increased to cause the coating to fall off, the fallen coating in the groove is cleaned, the coating is re-applied in the groove, and after curing, subsequent coating is carried out.