Sputtering plane silver-copper alloy target material and preparation method thereof

By melting and processing sterling silver and pure copper under a protective gas atmosphere, the problem of insufficient density and uniformity of alloy targets is solved, and silver-copper alloy targets with high density and uniformity are prepared, which improves the coating Stability and sputtering properties.

CN119082676APending Publication Date: 2024-12-06WUHU YINGRI TECH CO LTD
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202411145345.6
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-20
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The density and structural uniformity of alloy targets in existing low-radiation coating glasses are poor, affecting the stability and performance of the coating.

Method used

Smelting, casting and deposition, homogenizing annealing, total rolling, low-temperature annealing, machining CNC, binding and flaw detection treatment under a protective gas atmosphere, reducing the introduction of impurities and improving the density of alloy targets and uniformity.

Benefits of technology

The silver-copper alloy target prepared by this method has uniform composition and uniform grain distribution, which improves the thickness uniformity and sputtering rate of the coating to meet the sputtering needs.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082676A_ABST
    Figure CN119082676A_ABST
Patent Text Reader

Abstract

The invention relates to the technical field of metal target production, in particular to a sputtering plane silver-copper alloy target and a preparation method thereof.The preparation method comprises the steps that pure silver and pure copper are smelted in the atmosphere of protective gas, and liquid alloy is obtained; under the atmosphere of protective gas, the liquid alloy is subjected to heat preservation and pouring deposition in sequence, cooling is conducted after vacuum breaking, and a silver-copper alloy cast ingot is obtained; the silver-copper alloy ingot is sequentially subjected to homogenizing annealing, total rolling and low-temperature annealing, and then a silver-copper alloy coarse ingot is obtained; and the silver-copper alloy rough ingot is sequentially subjected to machining CNC, binding, flaw detection and aftertreatment, and the silver-copper alloy target material is obtained. According to the method, the silver-copper alloy coarse ingot is uniform in component, and the compactness is improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of metal target material production, and in particular to a sputtering plane silver-copper alloy target material and a preparation method thereof. Background Art

[0002] Low-emissivity coated glass is a coated glass with a thin film of metal or metal compound with low-emissivity function coated on the surface of the glass, which makes the glass surface have extremely high far-infrared reflectivity, thereby achieving the purpose of thermal insulation, and at the same time has sunshade and heat insulation effects.

[0003] In the existing technology, low-emissivity films are basically prepared by magnetron sputtering. Traditional low-emissivity coated glass is based on a very thin single or double silver film layer, which is sandwiched between two anti-reflective metal oxide protective layers to prevent oxidation and sulfidation of the silver layer, so as to stabilize the performance of the product and meet the color and other requirements of the product. In addition, in order to further protect the silver film layer and avoid erosion of the silver film layer in the subsequent sputtering reaction process, an alloy target material is added on one side of the silver film layer to act as a barrier layer. The density and uniformity of the alloy target material are important parameters to ensure the stability of the coating.

[0004] During the processing of alloy targets, some existing products have holes in their tissues and have poor density. For example, a publication number CN116334548A was disclosed on June 27, 2023, and its name is a silver-copper-zinc alloy sputtering target and a preparation method thereof. The silver-copper-zinc alloy sputtering target is composed of alloy components including Cu, Zn, Ni and balance silver. The obtained raw materials are smelted, refined and degassed; the alloy liquid obtained after degassing is cast using a cast iron mold to obtain a billet, and the obtained billet is hot rolled, homogenized heat treated and artificially aged in turn. After aging, it is taken out and water-cooled to obtain a silver-copper-zinc alloy sputtering target. This method can uniformly organize the target; but the amount of alloy is large and the impurity elements are relatively increased, which reduces the density and tissue uniformity of the alloy target. Summary of the invention

[0005] In view of this, the object of the present invention is to provide a sputtering planar silver-copper alloy target and a preparation method thereof to solve the problem of poor density.

[0006] Based on the above purpose, the present invention provides a method for preparing a sputtering planar silver-copper alloy target.

[0007] Pure silver and pure copper are melted in an atmosphere of protective gas to obtain a liquid alloy;

[0008] In an atmosphere of protective gas, the liquid alloy is sequentially subjected to heat preservation and pouring deposition, and after breaking the vacuum, it is cooled to obtain a silver-copper alloy ingot;

[0009] The silver-copper alloy ingot is subjected to homogenization annealing, total rolling, and low-temperature annealing in sequence, thereby obtaining a silver-copper alloy crude ingot;

[0010] The silver-copper alloy rough ingot is subjected to CNC machining, binding, flaw detection and post-processing in sequence to obtain the silver-copper alloy target.

[0011] Optionally, the mass ratio of pure copper to pure silver ranges from 10%:90% to 60%:40%.

[0012] Optionally, the smelting includes: adding pure silver and pure copper into a vacuum medium frequency induction melting furnace, and when the vacuum degree in the melting furnace ranges from 0.2Pa to 0.8Pa, raising the temperature to 1160°C to 1300°C, and keeping the temperature for 5min to 20min.

[0013] Optionally, the protective gas is argon, and the gas pressure range of the argon is 0.7 MPa to 0.9 MPa.

[0014] Optionally, the temperature range of the homogenization annealing is 600° C. to 800° C., and the insulation range is 2 h to 3 h.

[0015] Optionally, the total rolling includes hot rolling and cold rolling, the hot rolling process has a pass range of 10 to 20 times, the cold rolling process has a pass range of 1 to 5 times, and both the hot rolling and the cold rolling are performed by reciprocating rolling in a two-roll mill.

[0016] Optionally, the deformation amount of each pass of the hot rolling treatment ranges from 15% to 30%, the total deformation amount of the hot rolling is not less than 60%, and the deformation amount of each pass of the cold rolling treatment ranges from 10% to 20%.

[0017] Optionally, the CNC machining is to perform milling on the surface of the silver-copper alloy rough ingot to obtain the pre-target material.

[0018] Optionally, the binding includes: bonding the copper back plate and the pre-target material using a bonding material in a heated state.

[0019] A sputtering planar silver-copper alloy target is prepared by the above preparation method.

[0020] The beneficial effects of the present invention are as follows: the present invention provides a method for preparing a sputtering planar silver-copper alloy target material, which only uses pure silver and pure copper for smelting, reduces the introduction of impurity elements, effectively improves the density and uniformity of the silver-copper alloy target material structure by adopting a smelting and pouring treatment, and homogenizes the composition of the alloy target ingot, eliminates component segregation and structural inhomogeneity by adopting a homogenizing annealing treatment; the composition of the silver-copper alloy target material is uniform and the grain distribution is uniform by total rolling and low-temperature annealing; the composition of the silver-copper alloy target material is uniform and has a high density by machining CNC, binding, flaw detection, post-processing, etc., and the silver-copper alloy target material prepared by the present invention has a uniform coating thickness and a fast sputtering rate during sputtering, which fully meets the sputtering requirements. BRIEF DESCRIPTION OF THE DRAWINGS

[0021] In order to more clearly illustrate the embodiments of the present invention or the technical solutions in the prior art, the drawings required for use in the embodiments or the description of the prior art will be briefly introduced below. Obviously, the drawings described below are only embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without paying creative work.

[0022] Figure 1 The metallographic structure diagram of the sputtering planar silver-copper alloy target material prepared by the implementation of the present invention. DETAILED DESCRIPTION

[0023] In order to make the objectives, technical solutions and advantages of the present invention more clearly understood, the present invention is further described in detail below in conjunction with specific embodiments and with reference to the accompanying drawings.

[0024] It should be noted that, unless otherwise defined, the technical terms or scientific terms used in the embodiments of the present invention should be understood by people with ordinary skills in the field to which the present invention belongs. The "first", "second" and similar words used in the present invention do not represent any order, quantity or importance, but are only used to distinguish different components. "Including" or "comprising" and similar words mean that the elements or objects appearing before the word cover the elements or objects listed after the word and their equivalents, without excluding other elements or objects. "Connecting" or "connected" and similar words are not limited to physical or mechanical connections, but can include electrical connections, whether direct or indirect. "Up", "down", "left", "right" and the like are only used to indicate relative positional relationships. When the absolute position of the described object changes, the relative positional relationship may also change accordingly.

[0025] A method for preparing a sputtering planar silver-copper alloy target.

[0026] Pure silver and pure copper are melted in an atmosphere of protective gas to obtain a liquid alloy;

[0027] In an atmosphere of protective gas, the liquid alloy is sequentially subjected to heat preservation and pouring deposition, and after breaking the vacuum, it is cooled to obtain a silver-copper alloy ingot;

[0028] The silver-copper alloy ingot is subjected to homogenization annealing, total rolling, and low-temperature annealing in sequence, thereby obtaining a silver-copper alloy crude ingot;

[0029] The silver-copper alloy crude ingot is subjected to CNC machining, binding, flaw detection and post-processing in sequence to make the composition of the silver-copper alloy crude ingot uniform and improve the density to obtain the silver-copper alloy target.

[0030] The method only uses pure silver and pure copper for smelting, reduces the introduction of impurity elements, effectively improves the density and uniformity of the silver-copper alloy target material structure by adopting smelting and pouring treatment, and makes the composition of the alloy target ingot uniform, eliminates component segregation and structural inhomogeneity by adopting homogenization annealing treatment; makes the composition of the silver-copper alloy target material uniform and the grain distribution uniform by total rolling and low-temperature annealing; makes the composition of the silver-copper alloy target material uniform and has high density by machining CNC, binding, flaw detection, post-processing, etc.

[0031] The mass ratio of pure copper to pure silver ranges from 10%:90% to 60%:40%.

[0032] The purity of the pure copper is not less than 99.995%, and the purity of the pure silver is not less than 99.99%.

[0033] The smelting comprises: adding pure silver and pure copper into a vacuum medium frequency induction melting furnace, and when the vacuum degree in the melting furnace is in the range of 0.2Pa to 0.8Pa, raising the temperature to 1160°C to 1300°C, and keeping the temperature for 5min to 20min. The mechanical properties and anti-electromigration ability of the alloy target obtained by adding silver element to copper are significantly improved compared with the pure copper target, and the silver-copper alloy has good corrosion resistance, which effectively improves the density and uniformity of the silver-copper alloy target structure.

[0034] The protective gas may be argon gas, and the gas pressure of the argon gas ranges from 0.7 MPa to 0.9 MPa, and the gas pressure of the argon gas is preferably 0.8 MPa.

[0035] The temperature range of the homogenization annealing is 600°C to 800°C, and the holding time range is 2h to 3h, wherein the temperature is preferably 720°C, and the holding time is preferably 2h. The homogenization annealing process is used to homogenize the composition of the alloy ingot and eliminate composition segregation and organizational inhomogeneity.

[0036] The total rolling includes hot rolling and cold rolling. The number of passes of the hot rolling treatment ranges from 10 to 20 times, wherein the number of passes of the hot rolling treatment preferably ranges from 10 to 12 times. The number of passes of the cold rolling treatment ranges from 1 to 5 times, wherein the number of passes of the cold rolling treatment preferably ranges from 1 to 3 times. The hot rolling and cold rolling both adopt reciprocating rolling in a two-roll mill. The total rolling makes the silver-copper alloy target material uniform in composition and grain distribution.

[0037] The deformation range of the hot rolling process is 15% to 30%, preferably 20% to 25%, the total deformation is not less than 60%, preferably 70% to 80%, and the total deformation can be 60%, 70% or 80%.

[0038] The range of deformation amount per pass of the cold rolling treatment is 10% to 20%, and the range of deformation amount per pass of the cold rolling treatment is preferably 10% to 15%.

[0039] The temperature range of the low-temperature annealing is 400°C to 500°C, the temperature of the low-temperature annealing is preferably 450°C, and the holding time of the low-temperature annealing is 1h to 3h. The low-temperature annealing process is used to effectively eliminate or reduce the internal stress of the silver-copper alloy ingot, thereby obtaining a silver-copper alloy crude ingot.

[0040] The machining CNC is to perform milling on the surface of the silver-copper alloy rough ingot to obtain the pre-target material. The processing amount of the milling process ranges from 0.5mm to 2mm, and the processing amount of the milling process is preferably 0.7mm.

[0041] The binding includes: in a heated state, using a bonding material to bond the copper back plate to the pre-target material to obtain a middle target material, so that the pre-target material and the copper back plate are fully bonded, while applying ultrasonic vibration using an ultrasonic soldering iron equipped with a heater, while applying the bonding material, that is, arranging the bonding material in a molten state between the heated copper back plate and the pre-target material. Through metallization, the removal of dirt on the surfaces of the copper back plate and the pre-target material, the reduction of the oxide film, the removal of bubbles, etc. can be promoted, and the bonding material can be integrated into the surfaces of the copper back plate and the pre-target material, so that the target material and the copper back plate can be fully bonded together.

[0042] The flaw detection process is to use a flat metal target ultrasonic flaw detector to perform a welding rate flaw detection on the target material to obtain the rear target material, and the flaw detection welding rate is ≥90%, and the flaw detection welding rate is preferably 95%.

[0043] The post-treatment is to first use a scouring pad to clean the surface of the rear target material, and then use a roughness tester to detect the roughness of the surface of the rear target material. When the roughness Ra≤3.2, a silver-copper alloy target material is obtained, and the roughness is preferably 0.45.

[0044] A sputtering planar silver-copper alloy target is prepared by the above preparation method.

[0045] Embodiment 1

[0046] Select pure copper with a purity of 99.995% and pure silver with a purity of 99.99%, add the two into a vacuum medium frequency induction melting furnace in a ratio of 60% by mass of pure silver and 40% by mass of pure copper, and add the two into a vacuum medium frequency induction melting furnace with a protective gas. When the vacuum degree reaches 0.6 Pa, power is turned on and the temperature is raised. When the temperature reaches 1200°C, the alloy is melted into a liquid alloy.

[0047] In a protective gas having a protective gas pressure of 0.8 MPa, the liquid alloy is poured and deposited for 10 minutes, and the silver-copper alloy ingot is obtained by cooling after breaking the vacuum;

[0048] The silver-copper alloy ingot is subjected to high temperature homogenization annealing, the temperature is controlled at 720°C, and the temperature is kept for 2 hours;

[0049] The silver-copper alloy ingot which has been homogenized and annealed is placed on a two-roll rolling mill for 11 passes of reciprocating hot rolling, the deformation of each hot rolling pass is 20%, and the total deformation of the hot rolling is 78%, and then the temperature is lowered to 620°C, the holding time is 1.5h, and the silver-copper alloy ingot which has been hot rolled is cold rolled again for one pass of reciprocating cold rolling;

[0050] After cold rolling, the silver-copper alloy ingot is subjected to low-temperature annealing, the temperature is controlled at 450°C, and the heat preservation time is 1h to obtain a silver-copper alloy crude ingot;

[0051] The surface of the silver-copper alloy rough ingot is subjected to CNC milling processing to obtain the pre-target material;

[0052] Under the heating state, the pre-target material is bonded to the copper back plate using a bonding material to obtain a middle target material;

[0053] A flat metal target ultrasonic flaw detector is used to perform welding rate flaw detection on the target material to obtain a rear target material, wherein the welding rate of the flaw detection is ≥90%;

[0054] The surface of the rear target material is cleaned with a scouring pad, and then the roughness of the rear target material surface is tested using a roughness tester. When the roughness Ra≤3.2, a silver-copper alloy target material is obtained, and the average grain size of the silver-copper alloy target material is 50um.

[0055] Figure 1 The metallographic structure diagram of the silver-copper alloy target prepared in Example 1 is shown in FIG. Figure 1 It can be seen that the grains are evenly distributed, the composition is uniform, and the density is high.

[0056] Those skilled in the art should understand that the discussion of any of the above embodiments is merely illustrative and is not intended to imply that the scope of the present invention is limited to these examples. Under the concept of the present invention, the technical features in the above embodiments or different embodiments may be combined, the steps may be implemented in any order, and there are many other variations of the different aspects of the present invention as described above, which are not provided in detail for the sake of simplicity.

[0057] The embodiments of the present invention are intended to cover all such substitutions, modifications and variations that fall within the broad scope of the appended claims. Therefore, any omissions, modifications, equivalent substitutions, improvements, etc. made within the spirit and principles of the present invention should be included in the protection scope of the present invention.

Claims

1. A method for preparing a sputtering planar silver-copper alloy target, characterized in that: Pure silver and pure copper are melted in an atmosphere of protective gas to obtain a liquid alloy; In an atmosphere of protective gas, the liquid alloy is sequentially subjected to heat preservation and pouring deposition, and after breaking the vacuum, it is cooled to obtain a silver-copper alloy ingot; The silver-copper alloy ingot is subjected to homogenization annealing, total rolling, and low-temperature annealing in sequence, thereby obtaining a silver-copper alloy crude ingot; The silver-copper alloy rough ingot is subjected to CNC machining, binding, flaw detection and post-processing in sequence to obtain the silver-copper alloy target.

2. The method for preparing a sputtering planar silver-copper alloy target according to claim 1, characterized in that: The mass ratio of pure copper to pure silver ranges from 10%:90% to 60%:40%.

3. The method for preparing a sputtering planar silver-copper alloy target according to claim 1, characterized in that: The smelting comprises: adding pure silver and pure copper into a vacuum medium frequency induction melting furnace, and when the vacuum degree in the melting furnace ranges from 0.2Pa to 0.8Pa, raising the temperature to 1160°C to 1300°C, and keeping the temperature for 5min to 20min.

4. The method for preparing a sputtering planar silver-copper alloy target according to claim 1, characterized in that: The protective gas is argon gas, and the gas pressure of the argon gas ranges from 0.7 MPa to 0.9 MPa.

5. The method for preparing a sputtering planar silver-copper alloy target according to claim 1, characterized in that: The temperature range of the homogenization annealing is 600° C. to 800° C., and the heat preservation range is 2h to 3h.

6. The method for preparing a sputtering planar silver-copper alloy target according to claim 1, characterized in that: The total rolling includes hot rolling and cold rolling. The hot rolling process has a pass range of 10 to 20 times, and the cold rolling process has a pass range of 1 to 5 times. Both the hot rolling and the cold rolling are performed by reciprocating rolling in a two-roll mill.

7. The method for preparing a sputtering planar silver-copper alloy target according to claim 6, characterized in that: The deformation amount of each pass of the hot rolling treatment ranges from 15% to 30%, the total deformation amount of the hot rolling is not less than 60%, and the deformation amount of each pass of the cold rolling treatment ranges from 10% to 20%.

8. The method for preparing a sputtering planar silver-copper alloy target according to claim 1, characterized in that: The CNC machining is to perform milling on the surface of the silver-copper alloy rough ingot to obtain the pre-target material.

9. The method for preparing a sputtering planar silver-copper alloy target according to claim 8, characterized in that: The binding comprises: bonding the copper back plate and the pre-target material by using a bonding material in a heated state.

10. A sputtering planar silver-copper alloy target, characterized in that: Prepared by the method of claim 1.