Laminated structure coating with ceramic skeleton filled with sheet metal and preparation method of laminated structure coating

By forming a ceramic skeleton on the surface of carbon steel, the problems of poor shear resistance and low interface bonding strength in ceramic/metal multilayer film are solved, and high strength, toughness and good resistance are achieved Shearing capability improves surface mechanical properties.

CN119082731AActive Publication Date: 2024-12-06XIAN UNIV OF TECH
View PDF 9 Cites 0 Cited by

Patent Information

Application Number
CN202411182077.5
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-08-27
Publication Date
2024-12-06
Estimated Expiration
2044-08-27

AI Technical Summary

Technical Problem

The metal layer isolation structure of the existing ceramic/metal multilayer films leads to poor shear resistance and low interface bonding strength, which limits the improvement of surface mechanical properties.

Method used

A laminated structural coating with sheet metal filled with a ceramic skeleton on the surface of carbon steel is used to form a ceramic skeleton with high hardness and toughness through the first carburizing treatment and physical vapor deposition, and a sheet iron layer is filled therein. Realize metallurgical bonding and carbide in-situ precipitation of interlayer interfaces to enhance interface bonding strength.

Benefits of technology

The high strength, toughness and good shear resistance of the sheet metal laminated structure in the ceramic skeleton are realized, and the comprehensive mechanical properties of the surface are improved.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082731A_ABST
    Figure CN119082731A_ABST
Patent Text Reader

Abstract

The invention discloses a preparation method of a laminated structure coating with a ceramic skeleton filled with sheet metal, which comprises the following steps: (1) polishing the surface of carbon steel, and carburizing; (2) depositing a metal layer with a carbide forming ability on the surface of the carbon steel with the carburized layer, and alternately depositing a flaky iron layer and the metal layer with the carbide forming ability on the surface of the carbon steel by using a mask plate through a film layer preparation technology; (3) the carbon steel with the metal multi-layer structure coating on the surface is carburized, through the treatment, a laminated structure coating which takes ceramic as a framework and is filled with a flaky iron layer is formed on the surface of the carbon steel, the coating is high in ceramic phase volume fraction, compact and non-porous, an interlayer interface has a microcosmic irregular shape, metallurgical bonding is achieved, and the hardness of the coating is improved; and the strength, toughness and shear resistance of the material are remarkably improved.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the technical field of metal material surface modification methods, relates to a carbon steel surface ceramic skeleton filled with a flaky metal laminated structure, and also relates to a method for preparing a coating of the carbon steel surface ceramic skeleton filled with a flaky metal laminated structure. Background Art

[0002] At present, preparing ceramic / metal multilayer films on the surface of carbon steel is an effective method to improve its surface toughness. This multilayer film is a thin film formed by alternating hard ceramic layers and metal layers with good plasticity and toughness. However, the structure in which the metal layer isolates the ceramic layer restricts its shear resistance.

[0003] At present, the preparation technologies of ceramic / metal multilayer films mainly include physical vapor deposition (PVD) and chemical vapor deposition (CVD). Physical vapor deposition technology has the advantages of precise control of film thickness and composition, wide application range, and environmental friendliness. Chemical vapor deposition has the advantages of high deposition rate, good winding performance, and controllable film composition. However, ceramic / metal multilayer films prepared by PVD and CVD technology generally lack obvious element interdiffusion at the interlayer interface and the film-substrate interface, which restricts the bonding strength of the interface and limits the further improvement of the comprehensive mechanical properties of the surface.

[0004] In summary, from the perspective of the structure of the ceramic / metal multilayer film, the structural feature of the metal layer isolating the ceramic layer restricts its shear resistance; from the perspective of the preparation method of the ceramic / metal multilayer film, the poor interface bonding strength of the multilayer film restricts the further improvement of the mechanical properties of the multilayer film. In response to the above problems, the present invention designs a laminated structure coating with a high-strength ceramic skeleton and containing flaky tough metal, and proposes a preparation method combining physical vapor deposition and carburizing, and finally obtains a film with both strength and toughness and good shear resistance. Summary of the invention

[0005] The present invention aims to provide a laminated structure coating with a ceramic skeleton filled with sheet metal on the surface of carbon steel, so as to solve the problem of poor shear resistance caused by the metal layer isolating the ceramic layer in the existing ceramic-metal multilayer film technology. On the other hand, the purpose of the present invention is to provide a method for preparing a laminated structure filled with sheet metal in a ceramic skeleton on the surface of carbon steel, so as to solve the problem of low interface bonding strength of the multilayer film in the existing technology.

[0006] The technical scheme of the coating adopted by the laminated structure of the ceramic skeleton filled with sheet metal in the present invention is that the carbon steel surface has a coating with a ceramic phase as the skeleton and the gaps in the ceramic skeleton filled with sheet iron layers.

[0007] The technical solution adopted by the method for preparing the laminated structure coating with flaky metals filled in a ceramic framework of the present invention is specifically implemented according to the following steps:

[0008] Step 1: Grind the surface of the carbon steel and then perform the first carburizing treatment to obtain carbon steel with a carburized layer;

[0009] Step 2: Depositing a metal layer having carbide-forming ability on the surface of the carbon steel having the carburized layer by using a film preparation process;

[0010] Step 3: placing a deposition mold on the metal layer formed in step 2, using the deposition mold to deposit a flaky iron layer through a film preparation process, removing the deposition mold to obtain the flaky iron layer, and using the film preparation process to deposit again on the flaky iron layer to form a metal layer with carbide-forming ability, repeating the above operation, depositing the flaky iron layer and the metal layer with carbide-forming ability multiple times, and forming a coating with a metal with carbide-forming ability as a skeleton and filled with the flaky iron layer on the surface of the carbon steel;

[0011] Step 4: Place the coating formed in step 3 into a carburizing furnace for a second carburizing treatment to obtain a laminated structure coating with flaky metals filled in a ceramic framework.

[0012] The present invention is also characterized in that: the first carburizing treatment in step 1 is one of solid carburizing, gas carburizing, vacuum carburizing, and plasma carburizing, and the temperature range of the first carburizing treatment is 800° C.-1000° C.;

[0013] The carburized layer thickness L in step 1 ranges from 10 μm to 200 μm;

[0014] The deposition thickness of the metal layer having carbide-forming ability in step 2 is 5 μm-50 μm;

[0015] The film preparation process in step 2 and step 3 is one of physical vapor deposition, chemical vapor deposition, and spraying. The metal having carbide-forming ability in step 2 and step 3 is a metal composed of any one of W, Mo, Cr, Ta, Nb, Ti, Zr, and V.

[0016] Step 3 is specifically implemented as follows: placing a deposition mold on the metal layer formed in step 2, the deposition mold comprising a first mask plate and a second mask plate, the graphic position of the first mask plate and the graphic position of the second mask plate are staggered, using the first mask plate to deposit a flaky iron layer through a film layer preparation process, removing the first mask plate to obtain a flaky iron layer, using the film layer preparation process to deposit the flaky iron layer again to form a metal layer with carbide forming ability, then using the second mask plate to deposit the flaky iron layer through a film layer preparation process, removing the second mask plate to obtain a flaky iron layer, using the film layer preparation process to deposit the flaky iron layer again to form a metal layer with carbide forming ability, repeating the above operation, depositing the flaky iron layer and the metal layer with carbide forming ability multiple times, and forming a coating with a metal with carbide forming ability as a skeleton and filled with the flaky iron layer on the surface of the carbon steel.

[0017] The hole size (diameter of the circular hole, side length of the square hole or hexagonal hole) of the deposition mold in step 3 is 20μm-100μm, the thickness of the flaky iron layer is 1μm-30μm, and the number of flaky iron layers is 2-10 layers; the metal layer with carbide-forming ability is made of the same material as in step 2, and the thickness of a single layer is 3μm-50μm. The thickness of the metal layer with carbide-forming ability and the flaky iron layer are independently controlled, and the number of flaky iron layers and the metal layer with carbide-forming ability is the same;

[0018] In step 3, the flaky iron layer includes a pure iron layer with a carbon content lower than 0.0218wt% and a carbon steel layer with a carbon content between 0.0218wt% and 2.0wt%.

[0019] The carburizing treatment in step 4 adopts a method selected from solid carburizing, gas carburizing, vacuum carburizing, plasma carburizing, and interstitial atom carburizing, and the carburizing temperature ranges from 900°C to 1200°C.

[0020] The beneficial effects of the present invention are:

[0021] (1) In a coating with a ceramic phase as a skeleton and filled with a flaky iron layer, the ceramic skeleton has high hardness, strength and rigidity, and the flaky iron layer is conducive to improving the toughness of the coating, so that the coating has the characteristics of both strength and toughness and good shear resistance;

[0022] (2) During the high temperature process, the interlayer interface elements diffuse into each other, forming a high-strength interlayer interface with metallurgical bonding. The interface between the ceramic layer and the sheet metal layer presents an irregular shape. Compared with a flat interface, this irregular interface can more effectively enhance the toughness of the material;

[0023] (3) Carbides precipitate in situ, which increases the grain boundary strength. Iron is dissolved in the carbide ceramic phase, so its growth rate is faster and it also has better toughness.

[0024] (4) Due to the high solid solubility of carbon in iron, the flaky iron layer can effectively promote the continuous diffusion of carbon inward and can also serve as a carbon source to promote the formation of carbide ceramic phase. BRIEF DESCRIPTION OF THE DRAWINGS

[0025] Figure 1 It is a schematic diagram of the thickness of the carburized layer in the method for preparing a laminated structure coating with a ceramic skeleton filled with sheet metals according to the present invention;

[0026] Figure 2 It is a schematic diagram of the cross-sectional structure of depositing a metal layer having carbide-forming ability on the surface of a carbon steel having a carburized layer in step 2 of the method for preparing a laminated structure coating having a ceramic skeleton filled with flaky metals according to the present invention;

[0027] Figure 3 It is a schematic structural diagram of a square mask plate in Example 2 of the method for preparing a laminated structure coating having a ceramic framework filled with sheet metals according to the present invention;

[0028] Figure 4 It is a schematic structural diagram of a circular mask plate in Example 3 of the method for preparing a laminated structure coating having a ceramic framework filled with sheet metals according to the present invention;

[0029] Figure 5 It is a schematic structural diagram of a hexagonal mask plate in Example 4 of the method for preparing a laminated structure coating having a ceramic framework filled with flaky metals according to the present invention;

[0030] Figure 6 It is a schematic cross-sectional structure diagram of a laminated structure coating of a ceramic framework filled with flaky metals according to the present invention, in which a mask plate is used to deposit a flaky iron layer;

[0031] Figure 7 It is a schematic diagram of a laminated structure coating in which a sheet metal is filled in a ceramic framework of the present invention, and a metal layer having carbide forming ability is deposited after removing the mask plate;

[0032] Figure 8 It is a schematic structural diagram of a laminated structure coating in which a flaky iron layer is filled in a ceramic framework of the present invention; DETAILED DESCRIPTION

[0033] The present invention is described in detail below with reference to the accompanying drawings and specific embodiments.

[0034] The present invention relates to a method for preparing a laminated structure coating in which a ceramic framework is filled with sheet metal. Figure 1-Figure 8 As shown, the specific implementation steps are as follows:

[0035] Step 1: Grinding the surface of carbon steel and performing the first carburizing treatment to obtain carbon steel with a carburized layer, wherein the carburized layer thickness L ranges from 10 μm to 200 μm, and the carbon content ranges from 0.8 wt% to 2.0 wt%. The first carburizing treatment method is one of solid carburizing, gas carburizing, vacuum carburizing, and plasma carburizing, and the temperature ranges from 800° C. to 1000° C. Preferably, gas carburizing is selected;

[0036] Step 2: depositing a metal layer with carbide-forming ability on the surface of the carbon steel with the carburized layer by a film preparation process, wherein the film preparation process includes one of physical vapor deposition, chemical vapor deposition, and spraying, and the deposition thickness of the metal layer with carbide-forming ability is 5-50 μm. Any one of W, Mo, Cr, Ta, Nb, Ti, Zr, and V can be used to form the metal layer with carbide-forming ability. Preferably, magnetron sputtering is used;

[0037] Step 3: placing a deposition mold on the metal layer formed in step 2, the deposition mold comprising a first mask plate and a second mask plate, the pattern position of the first mask plate and the pattern position of the second mask plate are staggered, using the first mask plate to deposit a flaky iron layer through a film layer preparation process, removing the first mask plate to obtain a flaky iron layer, using the film layer preparation process to deposit the flaky iron layer again to form a metal layer with carbide forming ability, then using the second mask plate to deposit the flaky iron layer through a film layer preparation process, removing the second mask plate to obtain a flaky iron layer, using the film layer preparation process to deposit the flaky iron layer again to form a metal layer with carbide forming ability, repeating the above operation, depositing the flaky iron layer and the metal layer with carbide forming ability multiple times, and forming a coating with a metal with carbide forming ability as a skeleton and filled with the flaky iron layer on the surface of the carbon steel. The hole size (diameter of circular hole, side length of square hole or hexagonal hole) of the first mask plate and the second mask plate is 20μm-100μm, the thickness of the flaky iron layer is 1μm-30μm, and the number of layers is 2-10; the metal layer with carbide-forming ability uses the same material as step 2, and the single layer thickness ranges from 3μm-50μm. In step 3, the thickness of each layer is independently controlled, and the number of layers of the flaky iron layer and the metal layer with carbide-forming ability is the same. The film preparation process includes one of physical vapor deposition, chemical vapor deposition, and spraying;

[0038] Step 4: Place the coating formed in step 3 into a carburizing furnace for a second carburizing treatment to obtain a laminated structure coating with flaky metals filled in a ceramic skeleton. The second carburizing is performed by a method selected from solid carburizing, gas carburizing, vacuum carburizing, plasma carburizing, and interstitial atom carburizing. The second carburizing temperature ranges from 900°C to 1200°C. Preferably, vacuum carburizing is selected.

[0039] In the preparation method of the laminated structure coating with sheet metal filled in the ceramic skeleton of the present invention: in step 1, the role of carburization is to increase the carbon content of the surface layer of carbon steel. Therefore, in the carburization process of step 4, not only the external carbon atoms diffuse into the laminated structure coating (i.e., inward carburization), but also the carbon atoms on the surface layer of the carbon steel substrate diffuse into the laminated structure coating (i.e., outward diffusion). In this way, the effect of bidirectional carburization is achieved, which can not only effectively increase the thickness of the carburized layer, but also refine the grains of carbides.

[0040] In the preparation method of the laminated structure coating with flaky metal filled in the ceramic skeleton of the present invention: the role of the flaky iron layer formed by the staggered first mask plate and the second mask plate in step 3 is to make the ceramic phase in the laminated structure coating form a three-dimensional skeleton, thereby improving the surface rigidity and shear resistance. The principle is that as the flaky iron layer is staggered and deposited, the metal layer with carbide forming ability is connected, and a ceramic skeleton is formed after carburizing. The flaky iron layer fills the gaps in the skeleton and forms a diffusion bond with the ceramic skeleton. Therefore, designing a structure with a ceramic phase as the skeleton and filled with a flaky iron layer is a feasible solution.

[0041] In the preparation method of the laminated structure coating with flaky metal filled in the ceramic skeleton of the present invention: in step 4, the role of the flaky iron layer in the carburizing process is to store and release carbon atoms, which helps to promote the continuous inward diffusion of carbon atoms, helps to increase the carbonization rate, can withstand high carburizing temperatures, and the iron layer is still a metal layer after carburizing.

[0042] In the preparation method of the laminated structure coating filled with sheet metal in the ceramic skeleton of the present invention: the role of step 4 can be divided into three aspects: first, the metal layer with carbide forming ability is converted into a ceramic layer; second, the elements at the interlayer interface are promoted to diffuse each other to form an interface with metallurgical bonding; third, carbides are formed in situ, the grain boundary bonding strength is high, the density is high, and the formation of columnar crystal structure can be avoided. At the same time, when carbides precipitate in the interdiffusion area, a microscopic irregular interlayer interface is formed. Compared with a straight interface, this interface can more effectively enhance the toughness of the coating.

[0043] Example 1

[0044] The laminated structure coating with flaky metal filled in a ceramic skeleton of this embodiment comprises a ceramic phase multi-layer structure skeleton and a flaky iron layer, wherein the ceramic phase skeleton is filled with the flaky iron layer.

[0045] Example 2

[0046] The preparation method of the laminated structure coating with sheet metal filled in the ceramic framework of this embodiment is specifically implemented according to the following steps:

[0047] Step 1: Grind the surface of the carbon steel and perform the first carburizing treatment to obtain carbon steel with a carburized layer;

[0048] The first carburizing treatment in step 1 is vacuum carburizing, the temperature range of the first carburizing treatment is 800° C., the first carburizing time is 40 hours, the carburizing layer thickness L of the carbon steel with a carburized layer in step 1 is 10 μm, and the carbon content is 0.8 wt%;

[0049] Step 2: using a film preparation process to deposit a metal layer having carbide-forming ability on the surface of the carbon steel having the carburized layer;

[0050] In step 2, the metal having carbide-forming ability is Ti, the film layer preparation process is chemical vapor deposition, and the thickness is 5 μm;

[0051] Step 3: placing a deposition mold on the metal layer formed in step 2, using the deposition mold to deposit a flaky iron layer through a film preparation process, the deposition mold uses a first mask plate, removing the first mask plate to obtain a flaky iron layer, using a film preparation process to deposit again on the flaky iron layer to form a metal layer with carbide forming ability, depositing the flaky iron layer and the metal layer with carbide forming ability, and forming a coating with a carbide-forming metal as a skeleton and filled with the flaky iron layer on the surface of the carbon steel

[0052] The aperture size of the first mask plate in step 3 is 20 μm, and the film preparation process adopts chemical vapor deposition. The single layer thickness of the metal layer with carbide forming ability is 3 μm, the number of layers is 1, the metal layer with carbide forming ability is Ti, the flaky iron layer is pure iron, the thickness is 1 μm, and the number of layers is 1;

[0053] Step 4: placing the carbon steel surface having a laminated structure coating with a ceramic skeleton filled with flaky iron layers obtained in step 3 into a carburizing furnace for a second carburizing treatment to obtain a carbon steel surface having a ceramic skeleton filled with flaky metal laminated structure material;

[0054] The second carburizing treatment described in step 4 adopts vacuum carburizing, the carburizing treatment temperature range is 900° C., and the second carburizing time is 40 hours.

[0055] Example 3

[0056] The preparation method of the laminated structure coating with sheet metal filled in the ceramic framework of this embodiment is specifically implemented according to the following steps:

[0057] Step 1: Grind the surface of the carbon steel and perform the first carburizing treatment to obtain carbon steel with a carburized layer;

[0058] The first carburizing treatment in step 1 is gas carburizing, the temperature of the first carburizing treatment is 900° C., the first carburizing time is 10 h, the carburizing layer thickness L of the carbon steel with a carburized layer in step 1 is 50 μm, and the carbon content is 1.2 wt%;

[0059] Step 2: using a film preparation process to deposit a metal layer having carbide-forming ability on the surface of the carbon steel having the carburized layer;

[0060] In step 2, the metal having carbide-forming ability is Zr, the film layer preparation process is physical vapor deposition, and the thickness is 10 μm;

[0061] A deposition mold is placed on the metal layer formed in step 2, wherein the deposition mold includes a first mask plate and a second mask plate, wherein the graphic position of the first mask plate is staggered with the graphic position of the second mask plate, and the flaky iron layer is deposited by a film layer preparation process using the first mask plate, and the first mask plate is removed to obtain the flaky iron layer, and the film layer preparation process is used to deposit the flaky iron layer again to form a metal layer with carbide forming ability on the flaky iron layer, and then the flaky iron layer is deposited by a film layer preparation process using the second mask plate, and the second mask plate is removed to obtain the flaky iron layer, and the film layer preparation process is used to deposit the metal layer with carbide forming ability on the flaky iron layer again to form a metal layer with carbide forming ability, and the above operation is repeated to deposit the flaky iron layer and the metal layer with carbide forming ability for multiple times, and the flaky iron layer fills the skeleton gap to form a coating on the carbon steel surface with the metal with carbide forming ability as the skeleton and filled with the flaky iron layer;

[0062] The aperture size of the first mask plate and the second mask plate in step 3 are both 50 μm, and the film preparation process adopts physical vapor deposition. The single layer thickness of the metal layer with carbide forming ability is 8 μm, and the number of layers is 6. The metal layer with carbide forming ability is selected from Zr, and the flaky iron layer is pure iron, with a thickness of 1.5 μm and 6 layers;

[0063] Step 4: placing the laminated structure coating having a flaky iron layer filled in a ceramic skeleton on the carbon steel surface obtained in step 3 into a carburizing furnace for a second carburizing treatment, thereby obtaining a laminated structure material having a flaky metal layer filled in a ceramic skeleton on the carbon steel surface, wherein the flaky iron layer formed by the misalignment of the first mask plate and the second mask plate is connected to the metal layer having carbide forming ability, and after the second carburizing, the flaky iron layer and the ceramic skeleton promote the mutual diffusion of elements at the interface between the layers, thereby forming an interface with metallurgical bonding;

[0064] The second carburizing treatment described in step 4 adopts plasma carburizing, the carburizing treatment temperature range is 1000° C., and the second carburizing time is 6 hours.

[0065] Example 4

[0066] The preparation method of the laminated structure coating with sheet metal filled in the ceramic framework of this embodiment is specifically implemented according to the following steps:

[0067] Step 1: Grind the surface of the carbon steel and perform the first carburizing treatment to obtain carbon steel with a carburized layer;

[0068] The first carburizing treatment in step 1 is solid carburizing, the temperature range of the first carburizing treatment is 1000° C., the first carburizing time is 5 hours, the carburizing layer thickness L of the carbon steel with a carburized layer in step 1 is 200 μm, and the carbon content is 2.0 wt%;

[0069] Step 2: using a film preparation process to deposit a metal layer having carbide-forming ability on the surface of the carbon steel having the carburized layer;

[0070] In step 2, the metal with carbide forming ability is W, the film layer preparation process is thermal spraying, and the thickness is 50 μm;

[0071] A deposition mold is placed on the metal layer formed in step 2, wherein the deposition mold includes a first mask plate and a second mask plate, wherein the graphic position of the first mask plate is staggered with the graphic position of the second mask plate, and a flaky iron layer is deposited by a film layer preparation process using the first mask plate, and the first mask plate is removed to obtain a flaky iron layer, and a metal layer having carbide forming ability is deposited again on the flaky iron layer by a film layer preparation process, and the flaky iron layer is deposited by a second mask plate by a film layer preparation process, and the second mask plate is removed to obtain a flaky iron layer, and a metal layer having carbide forming ability is deposited again on the flaky iron layer by a film layer preparation process, and the above operation is repeated, and the flaky iron layer and the metal layer having carbide forming ability are deposited multiple times, so as to form a coating having a metal having carbide forming ability as a skeleton and filling the flaky iron layer on the surface of the carbon steel;

[0072] The aperture size of the first mask plate and the second mask plate in step 3 is 100 μm, and the film layer preparation process adopts thermal spraying. The single layer thickness of the metal layer with carbide forming ability is 50 μm, and the number of layers is 10. The metal layer with carbide forming ability is W, and the flaky iron layer is carbon steel with a carbon content of 2.0wt%, and its thickness is 30 μm, and the number of layers is 10;

[0073] Step 4: placing the carbon steel surface having a laminated structure coating with a ceramic skeleton filled with flaky iron layers obtained in step 3 into a carburizing furnace for a second carburizing treatment to obtain a carbon steel surface having a ceramic skeleton filled with flaky metal laminated structure material;

[0074] The second carburizing treatment described in step 4 adopts vacuum carburizing, the carburizing treatment temperature range is 1200° C., and the second carburizing time is 2 hours.

[0075] The mechanical properties of the laminated structure coatings with sheet metal filled in the ceramic framework prepared in Examples 2-4 were tested, and the test results are shown in the following table:

[0076] project Fracture toughness Surface hardness Example 2 <![CDATA[8.6MPa·m 1 / 2 ]]> 2300HV Example 3 <![CDATA[8.2MPa·m 1 / 2 ]]> 2400HV Example 4 <![CDATA[12.4MPa·m 1 / 2 ]]> 2000HV

[0077] By the above method, the fracture toughness of the laminated structure coating of the present invention with the sheet metal filled in the ceramic framework exceeds 8MPa·m 1 / 2 , surface hardness exceeds 2000HV, and mechanical properties are good; the coating of the present invention uses a ceramic phase as a skeleton and is filled with a flaky iron layer. The ceramic skeleton has high hardness, strength and rigidity, and the flaky iron layer is beneficial to improving the toughness of the coating, so that the coating has the characteristics of both strength and toughness and good shear resistance.

Claims

1. A laminated coating with a ceramic framework filled with sheet metal, characterized in that: The carburized layer comprises a coating layer with a ceramic phase as a skeleton and flaky iron layers filling gaps in the ceramic skeleton.

2. A method for preparing a laminated structure coating with sheet metal filled in a ceramic framework, characterized in that: Follow the steps below to implement it: Step 1: Grind the surface of the carbon steel and then perform the first carburizing treatment to obtain carbon steel with a carburized layer; Step 2: using a film preparation process to deposit a metal layer having carbide-forming ability on the surface of the carbon steel having the carburized layer; Step 3: placing a deposition mold on the metal layer formed in step 2, using the deposition mold to deposit a flaky iron layer through a film preparation process, removing the deposition mold to obtain the flaky iron layer, and using the film preparation process to deposit again on the flaky iron layer to form a metal layer with carbide-forming ability, repeating the above operation, depositing the flaky iron layer and the metal layer with carbide-forming ability multiple times, and forming a coating with a metal with carbide-forming ability as a skeleton and filled with the flaky iron layer on the surface of the carbon steel; Step 4: Place the coating formed in step 3 into a carburizing furnace for a second carburizing treatment to obtain a laminated structure coating with flaky metals filled in a ceramic framework.

3. The method for preparing a laminated structure coating with sheet metal filled in a ceramic framework according to claim 2, characterized in that: The step 3 is specifically implemented as follows: A deposition mold is placed on the metal layer formed in step 2, the deposition mold comprising a first mask plate and a second mask plate, the graphic position of the first mask plate and the graphic position of the second mask plate are staggered, the flaky iron layer is deposited by a film layer preparation process using the first mask plate, the first mask plate is removed to obtain the flaky iron layer, the film layer preparation process is used to deposit the flaky iron layer again to form a metal layer with carbide forming ability on the flaky iron layer, the second mask plate is used to deposit the flaky iron layer by the film layer preparation process, the second mask plate is removed to obtain the flaky iron layer, the film layer preparation process is used to deposit the flaky iron layer again to form a metal layer with carbide forming ability on the flaky iron layer, the above operation is repeated, the flaky iron layer and the metal layer with carbide forming ability are deposited multiple times, and a coating with a metal with carbide forming ability as a skeleton and filled with the flaky iron layer is formed on the surface of the carbon steel.

4. The method for preparing a laminated structure coating with sheet metal filled in a ceramic framework according to claim 2, characterized in that: The first carburizing treatment method described in step 1 is one of solid carburizing, gas carburizing, vacuum carburizing, and plasma carburizing. The temperature range of the first carburizing treatment is 800° C.-1000° C., and the first carburizing time is 2h-40h.

5. The method for preparing a laminated structure coating with sheet metal filled in a ceramic framework according to claim 2, characterized in that: The carburized layer thickness L of the carbon steel with the carburized layer in step 1 is in the range of 10 μm-200 μm, and the carbon content is in the range of 0.8%-2.0%.

6. The method for preparing a laminated structure coating with sheet metal filled in a ceramic framework according to claim 2, characterized in that: The deposition thickness of the metal layer having carbide-forming ability in step 2 is 5 μm-50 μm.

7. The method for preparing a laminated structure coating with sheet metal filled in a ceramic framework according to claim 2, characterized in that: The film layer preparation process in step 2 and step 3 is one of physical vapor deposition, chemical vapor deposition, and spraying. The metal with carbide forming ability in step 2 and step 3 is a metal composed of any one of W, Mo, Cr, Ta, Nb, Ti, Zr, and V.

8. The method for preparing a laminated structure coating with sheet metal filled in a ceramic framework according to claim 2, characterized in that: In step 3, the pore size of the deposition mold is 20μm-100μm, the single layer thickness of the metal layer with carbide forming ability ranges from 3μm-50μm, the number of layers ranges from 2-10 layers, and the thickness of the flaky iron layer ranges from 1μm-30μm, and the number of layers ranges from 2-10 layers.

9. The method for preparing a laminated structure coating with sheet metal filled in a ceramic framework according to claim 2, characterized in that: The flaky iron layer in step 3 includes a pure flaky iron layer having a carbon content lower than 0.0218wt% and a carbon steel layer having a carbon content between 0.0218wt% and 2.0wt%.

10. The method for preparing a laminated structure coating with sheet metal filled in a ceramic framework according to claim 2, characterized in that: The second carburizing treatment described in step 4 adopts a method selected from solid carburizing, gas carburizing, vacuum carburizing, plasma carburizing, and interstitial atom carburizing. The temperature range of the second carburizing treatment is 900° C.-1200° C., and the second carburizing time is 2h-40h.

Citation Information

Patent Citations

  • Method for preparing ceramic multilayer film on metal surface by chemical heat treatment

    CN113621937A

  • Structure of carbon steel surface ceramic metal interlocking laminated material and preparation method thereof

    CN116604898A

  • Ceramic iron-nickel alloy double-bionic multilayer film structure and preparation method thereof

    CN116607097A

  • Method for preparing transition metal surface ceramic layer through iron layer medium carburization

    CN116607101A

  • Coating material and its production method

    JP2002180271A