Nickel-cobalt-iron Prussian blue seawater oxidation electrocatalyst rich in cyanide vacancies and preparation method of nickel-cobalt-iron Prussian blue seawater oxidation electrocatalyst

Low-temperature N2 plasma treatment introduces cyanide vacancies in nickel-cobalt-iron Prussian blue catalysts, addressing OER kinetics and seawater electrolysis challenges, achieving superior catalytic performance and stability.

CN119082770APending Publication Date: 2024-12-06QINGDAO UNIV OF SCI & TECH +1
View PDF 0 Cites 0 Cited by

Patent Information

Application Number
CN202410994583.8
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-07-24
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The oxygen evolution reaction (OER) in electrochemical water splitting is hindered by slow kinetics due to the complex four-electron redox process, and direct seawater electrolysis faces challenges from chlorine oxidation competing with OER, while Prussian blue analogs suffer from poor electrical conductivity and structural damage during high-temperature pyrolysis.

Method used

A low-temperature glow discharge N2 plasma treatment is applied to introduce cyanide vacancies in a nickel-cobalt-iron Prussian blue catalyst, forming an amorphous phase with a crystalline edge and an in-situ FeOOH layer, enhancing catalytic activity and stability in seawater.

Benefits of technology

The modified catalyst exhibits improved OER activity and durability in alkaline seawater, outperforming commercial RuO2 electrodes and maintaining catalyst integrity despite chloride ion corrosion.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082770A_ABST
    Figure CN119082770A_ABST
Patent Text Reader

Abstract

The invention discloses a Prussian blue (PBA)-based oxygen evolution electrocatalyst rich in cyanide vacancy as well as a preparation method and application of the Prussian blue-based oxygen evolution electrocatalyst. According to the method, NiCoFe-PBA is treated through low-temperature glow discharge N2 plasma, and the electrocatalyst rich in cyanide vacancies (N2-NiCoFe-PBA) is prepared. Rich cyanide vacancies can adjust the local electronic environment, the loss of [Fe (CN) 6] < 4-> in the PBA structure in the oxygen evolution process is inhibited, and the surface of N2-NiCoFe-PBA is favorably reconstructed into NiCoFe-OOH. The cyanide vacancy and the in-situ reconstructed FeOOH layer effectively inhibit corrosion of Cl <-> to the catalyst, and the durability of the catalyst in alkaline seawater is improved. In alkaline simulated seawater and an alkaline natural seawater solution, under the condition of 100 mA cm <-2 >, the N2-NiCoFe-PBA only needs the overpotential of 293 mV and the overpotential of 323mV respectively; even in a 2.0 mol / L high-salt alkaline solution, the catalyst can stably work for more than 100 hours under the large current density of 250 mA cm <-2 >, and the NiCoFe-PBA precursor can only stably operate for less than 3 hours.
Need to check novelty before this filing date? Find Prior Art

Description

Technical field:

[0001] The present invention belongs to the field of new energy material technology and electrochemical catalysis, and specifically relates to a nickel-cobalt-iron Prussian blue oxygen evolution electrocatalyst rich in cyanide vacancies; it also relates to a preparation method of the catalyst and its application in electrocatalytic pure water and seawater anodic oxygen evolution reaction. Background technology:

[0002] Electrochemical water splitting is considered an effective sustainable energy solution that can generate high-calorific hydrogen by storing intermittent renewable energy such as wind, solar and tidal energy. However, in this energy conversion process, compared with the two-electron hydrogen evolution reaction (HER), the oxygen evolution reaction (OER) exhibits slower kinetics due to the need to overcome the complex four-electron redox process to form the rigid O-O double bond, which determines the overall efficiency of water splitting. In recent years, efficient and stable electrocatalysts such as transition metal (hydr)oxides, selenides, phosphides, etc. have been shown to accelerate the OER process, and some of these catalysts even outperform the precious metal catalysts of IrO2 and RuO2.

[0003] Due to the scarcity of freshwater resources around the world, large-scale electrolysis of freshwater is very challenging, especially in coastal arid areas. Relatively speaking, seawater accounts for about 96.5% of global water resources and is an almost inexhaustible electrolyte raw material in the water electrolysis process. Direct electrolysis of seawater can both develop sustainable energy and solve the serious problems of water shortage and high freshwater demand in coastal arid areas. One of the biggest challenges in seawater electrolysis is Cl - Oxidation, including chlorine oxidation reaction (CER) in acidic electrolytes and hypochlorite (ClO - ), both of which will compete with OER during the reaction.

[0004] Prussian blue analogs (PBAs) are used as pre-catalysts for OER due to their unique porous structure and abundant redox centers. However, their poor electrical conductivity and intrinsic catalytic activity hinder their further application in catalytic oxidation in alkaline fresh water or seawater. Therefore, PBAs are usually converted into oxides, phosphides or sulfides by high-temperature pyrolysis. However, high-temperature pyrolysis usually leads to damage to the PBA framework and loss of well-distributed metal sites. Introducing vacancies is a common catalyst modification method. Vacancies can adjust the local electronic environment of metal sites while maintaining the original structure of the crystalline material, thereby enhancing catalytic activity and stability. The present invention creates CN vacancies (V in NiCoFe-PBA framework) by low-temperature glow discharge N2 plasma. CN) to activate the metal sites. Due to the lower treatment temperature and high energy activity, N2 plasma can achieve non-destructive modification of NiCoFe-PBA while retaining the PBA skeleton. In addition, the ternary PBA catalyst has better electrochemical activity than the bimetallic catalyst. The V-rich CN The electrocatalyst (N2-NiCoFe-PBA) exhibits better OER activity and durability than pristine NiCoFe-PBA.

[0005] The present invention uses low temperature glow discharge N2 plasma to convert V CN NiCoFe-PBA was introduced to prepare V-rich CN Electrocatalyst (N2-NiCoFe-PBA). V CN It can not only adjust the local electronic environment but also inhibit the [Fe(CN)6] 4- This is conducive to the reconstruction of the N2-NiCoFe-PBA surface into NiCoFe-OOH. CN The in-situ formed FeOOH capping layer can inhibit the Cl - The method can penetrate into the catalyst layer and improve the durability of the catalyst in seawater. This method has important theoretical and practical significance for the development of transition metal Prussian blue-based electrocatalysts and energy conversion and storage devices. Summary of the invention:

[0006] In view of the deficiencies in the prior art and the needs of research and application in this field, one of the objects of the present invention is to provide a Prussian blue-based oxygen evolution electrocatalyst rich in cyanide vacancies; the electrocatalyst is characterized in that the electrocatalyst is based on nickel foam, the nickel-cobalt-iron Prussian blue cube is an amorphous phase rich in cyanide vacancies along the diagonal, and the edge of the cube is a crystalline nickel-cobalt-iron Prussian blue phase; during the preparation process of the electrocatalyst, the concentration of cyanide vacancies is adjusted by controlling the nitrogen plasma voltage, and during the oxygen evolution process, the surface of the nickel-cobalt-iron Prussian blue will be in-situ converted into a NiCoFeOOH active phase; the cyanide vacancies are denoted as V CN ; Nickel-cobalt-iron Prussian blue is denoted as NiCoFe-PBA; the Prussian blue-based oxygen evolution electrocatalyst rich in cyanide vacancies is denoted as N2-NiCoFe-PBA; the catalyst without plasma treatment is denoted as NiCoFe-PBA.

[0007] The second object of the present invention is to provide a method for preparing a Prussian blue-based oxygen evolution electrocatalyst rich in cyanide vacancies, which specifically comprises the following steps:

[0008] (a) Preparation of NiCoFe-PBA

[0009] Three pieces of 2×3cm 2The nickel foam was ultrasonically treated with 1 mol / L hydrochloric acid solution, deionized water and ethanol for 30, 5 and 10 min respectively, and dried at 50°C for 6 h; 0.2181 g Ni(NO3)2·6H2O, 0.2183 g Co(NO3)2·6H2O and 0.6617 g Na3C6H5O7·2H2O were dissolved in 50 mL deionized water to form a clear solution A; 0.3293 g K3[Fe(CN)6] was dissolved in 50 mL deionized water to form a solution B; under magnetic stirring, solution B was slowly added to solution A to form a mixed solution C at room temperature; the pretreated nickel foam was soaked in the mixed solution C for 24 h, washed with deionized water and ethanol for 3 times respectively, and dried at 50°C overnight to obtain NiCoFe-PBA precursor;

[0010] (b) Preparation of N2-NiCoFe-PBA

[0011] The NiCoFe-PBA precursor prepared in step (a) is placed in a gas plasma chamber, the pressure in the chamber is kept below 0.8 mbar by reducing the pressure, N2 is introduced at a flow rate of 30 sccm, and after stabilization, an external voltage of 600 V to 900 V is applied, and air plasma treatment is performed for 5 to 40 minutes to obtain a N2-NiCoFe-PBA catalyst;

[0012] The prepared NiCoFe-PBA precursor is uniformly distributed nanocubes with a size of ~200nm and clear corners and edges; after N2 plasma activation, N2-NiCoFe-PBA retains the nanocube morphology well, but its surface becomes rougher than the NiCoFe-PBA precursor, and the cubes are transformed into an amorphous phase rich in cyanide vacancies along the diagonal, while the edges of the cubes are crystalline NiCoFe-PBA phase; during the OER process, a FeOOH protective layer is formed on the surface of N2-NiCoFe-PBA, which can effectively inhibit the corrosion of the catalyst and improve its stability and durability.

[0013] The third object of the present invention is to provide a Prussian blue-based oxygen evolution electrocatalyst rich in cyanide vacancies, characterized in that the catalyst is used for the anodic oxygen evolution reaction in alkaline simulated seawater and alkaline natural seawater.

[0014] The present invention prepares a V-rich NiCoFe-PBA by treating the trimetallic NiCoFe-PBA with low temperature glow discharge N2 plasma. CN The catalyst N2-NiCoFe-PBA has unsaturated catalytic sites due to its rich defects, which effectively reduces the overpotential of OER. CN It can effectively inhibit [Fe(CN)6] 4-The loss of FeOOH in situ and the nanocube skeleton are maintained, and the surface is reconstructed into NiCoFe-OOH in situ, in which the in situ generated FeOOH protective layer and V CN It can effectively inhibit the corrosion of chloride ions in seawater media and inhibit the dissolution and leaching of catalysts, thereby improving the OER catalytic activity and stability in alkaline simulated seawater and alkaline natural seawater.

[0015] Compared with the prior art, the present invention has the following main advantages and beneficial effects:

[0016] 1) The OER electrocatalyst of the present invention is a non-precious metal material prepared by low-temperature glow discharge plasma. The raw materials used are easy to purchase, abundant in resources and low in cost. The method is low-temperature and non-destructive, and is more energy-saving than traditional high-temperature treatment, and is convenient for large-scale production;

[0017] 2) The present invention has a rich V CN The unsaturated catalytic sites produced by the Prussian blue-based oxygen evolution electrocatalyst are rich in defects, which effectively reduce the overpotential of OER. The OER catalytic activity and stability in alkaline simulated seawater and alkaline natural seawater are better than most non-precious metal catalysts reported in current research.

[0018] 3) The present invention has a rich V CN The Prussian blue-based oxygen evolution electrocatalyst has better electrochemical performance than the commercial RuO2 electrode in the field of OER catalysis.

[0019] 4) The present invention provides a novel catalyst and electrocatalyst synthesis idea for seawater electrolysis. Description of the drawings:

[0020] Figure 1 They are respectively the scanning electron microscope images of NiCoFe-PBA (A) obtained in comparative example 1, the N2-NiCoFe-PBA (B) obtained in example 1, and the transmission electron microscope images of N2-NiCoFe-PBA (C) obtained in example 1.

[0021] Figure 2 XRD diagrams of NiCoFe-PBA obtained in Comparative Example 1 and N2-NiCoFe-PBA obtained in Example 1.

[0022] Figure 3 Comparative Example 1, Comparative Example 2, ... -1 Linear sweep voltammogram of OER in KOH solution.

[0023] Figure 4The catalysts N2-NiCoFe-PBA, N2-NiCoFe-PBA-600, N2-NiCoFe-PBA-700 and N2-NiCoFe-PBA-900 obtained in Example 1, Example 2, Example 3 and Example 4 were heated to 1.0 mol L -1 Linear sweep voltammogram of OER in KOH solution.

[0024] Figure 5 The catalysts N2-NiFe-PBA, N2-NiFe-PBA-600, N2-NiFe-PBA-700 and N2-NiFe-PBA-900 obtained in Example 5, Example 6, Example 7 and Example 8 were heated to 1.0 mol L -1 Linear sweep voltammogram of OER in KOH solution.

[0025] Figure 6 The catalysts N2-CoFe-PBA, N2-CoFe-PBA-600, N2-CoFe-PBA-700 and N2-CoFe-PBA-900 obtained in Example 9, Example 10, Example 11 and Example 12 were heated to 1.0 mol L -1 Linear sweep voltammogram of OER in KOH solution.

[0026] Figure 7 The catalysts N2-NiCoFe-PBA, N2-NiFe-PBA, N2-CoFe-PBA, NiCoFe-PBA, NiFe-PBA, CoFe-PBA obtained in Example 1, Example 5, Example 9, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were quenched at 1.0 mol L -1 Linear sweep voltammogram of OER in KOH.

[0027] Figure 8 The catalysts N2-NiCoFe-PBA and NiCoFe-PBA obtained in Example 1 and Comparative Example 1 were - 1 KOH + 0.5 mol L -1 Linear sweep voltammogram of OER in NaCl mixed solution.

[0028] Fig. 9 The catalysts N2-NiCoFe-PBA and NiCoFe-PBA obtained in Example 1 and Comparative Example 1 were - 1 Linear sweep voltammogram of OER in KOH+natural seawater mixed solution.

[0029] Fig.10The catalyst N2-NiCoFe-PBA obtained in Example 1 was added at 1.0 mol L -1 Stepwise chronopotentiogram (a) and constant current chronopotentiogram (b) in KOH.

[0030] Fig.11 The catalysts N2-NiCoFe-PBA and NiCoFe-PBA obtained in Example 1 and Comparative Example 1 were quenched in 1.0 mol L - 1 KOH + 0.5 mol L -1 Constant current chronopotentiometry curves in NaCl mixed solution.

[0031] Fig.12 The N2-NiCoFe-PBA (A and B) obtained in Example 1 and the NiCoFe-PBA (C and D) obtained in Comparative Example 1 were heated to 1.0 mol L -1 KOH + 0.5 mol L -1 Scanning electron microscopy image after 24h stability test in NaCl mixed solution.

[0032] Fig.13 The N2-NiCoFe-PBA obtained in Example 1 was added to 1.0 mol L -1 Constant current chronopotentiometry curves in KOH+natural seawater (a), N2-NiCoFe-PBA obtained in Example 1 and NiCoFe-PBA obtained in Comparative Example 1 at 1.0 mol L -1 KOH+2molL -1 Constant current chronopotentiometry curve in NaCl mixed solution (b). Specific implementation method:

[0033] For a further understanding of the present invention, the present invention is further described below in conjunction with the accompanying drawings and embodiments, but the present invention is not limited in any way.

[0034] Embodiment 1:

[0035] (a) Preparation of NiCoFe-PBA

[0036] Three pieces of 2×3cm 2The nickel foam was ultrasonically treated with 1 mol / L hydrochloric acid solution, deionized water and ethanol for 30, 5 and 10 min, respectively, and dried at 50°C for 6 h; 0.2181 g Ni(NO3)2·6H2O, 0.2183 g Co(NO3)2·6H2O and 0.6617 g Na3C6H5O7·2H2O were dissolved in 50 mL deionized water to form a clear solution A; 0.3293 g K3[Fe(CN)6] was dissolved in 50 mL deionized water to form a solution B; under magnetic stirring, solution B was slowly added to solution A to form a mixed solution C at room temperature; the pretreated nickel foam was soaked in the mixed solution C for 24 h, washed with deionized water and ethanol for 3 times, respectively, and dried at 50°C overnight to obtain a NiCoFe-PBA precursor.

[0037] (b) Preparation of N2-NiCoFe-PBA

[0038] The NiCoFe-PBA precursor prepared in step (a) was placed in a gas plasma chamber, and the pressure in the chamber was maintained below 0.8 mbar by reducing the vacuum pressure. N2 was introduced at a flow rate of 30 sccm. After stabilization, an external voltage of 800 V was applied, and air plasma treatment was performed for 10 minutes to obtain a N2-NiCoFe-PBA catalyst.

[0039] Embodiment 2:

[0040] (a) Preparation of NiCoFe-PBA

[0041] Prepared according to the method and conditions of step (a) in Example 1.

[0042] (b) Preparation of N2-NiCoFe-PBA

[0043] The NiCoFe-PBA precursor prepared in step (a) was placed in a gas plasma chamber, the pressure in the chamber was kept below 0.8 mbar under reduced pressure, N2 was introduced at a flow rate of 30 sccm, and after stabilization, an external voltage of 600 V was applied, and air plasma treatment was performed for 10 minutes to obtain N2-NiCoFe-PBA-600 catalyst.

[0044] Embodiment 3:

[0045] (a) Preparation of NiCoFe-PBA

[0046] Prepared according to the method and conditions of step (a) in Example 1.

[0047] (b) Preparation of N2-NiCoFe-PBA

[0048] The NiCoFe-PBA precursor prepared in step (a) was placed in a gas plasma chamber, and the pressure in the chamber was maintained below 0.8 mbar under reduced pressure. N2 was introduced at a flow rate of 30 sccm. After stabilization, an external voltage of 700 V was applied, and air plasma treatment was performed for 10 minutes to obtain N2-NiCoFe-PBA-700 catalyst.

[0049] Embodiment 4:

[0050] (a) Preparation of NiCoFe-PBA

[0051] Prepared according to the method and conditions of step (a) in Example 1.

[0052] (b) Preparation of N2-NiCoFe-PBA

[0053] The NiCoFe-PBA precursor prepared in step (a) was placed in a gas plasma chamber, and the pressure in the chamber was maintained below 0.8 mbar under reduced pressure. N2 was introduced at a flow rate of 30 sccm. After stabilization, an external voltage of 900 V was applied, and air plasma treatment was performed for 10 minutes to obtain N2-NiCoFe-PBA-900 catalyst.

[0054] Embodiment 5:

[0055] (a) Preparation of NiFe-PBA

[0056] Three pieces of 2×3cm 2 The nickel foam was ultrasonically treated with 1 mol / L hydrochloric acid solution, deionized water and ethanol for 30, 5 and 10 min, respectively, and dried at 50°C for 6 h; 0.4362 g Ni(NO3)2·6H2O and 0.6617 g Na3C6H5O7·2H2O were dissolved in 50 mL deionized water to form a clear solution A; 0.3293 g K3[Fe(CN)6] was dissolved in 50 mL deionized water to form a solution B; under magnetic stirring, solution B was slowly added to solution A to form a mixed solution C at room temperature; the pretreated nickel foam was soaked in the mixed solution C for 24 h, washed with deionized water and ethanol for 3 times, respectively, and dried at 50°C overnight to obtain a NiFe-PBA precursor.

[0057] (b) Preparation of N2-NiFe-PBA

[0058] The NiFe-PBA precursor prepared in step (a) was placed in a gas plasma chamber, and the pressure in the chamber was maintained below 0.8 mbar by reducing the vacuum. N2 was introduced at a flow rate of 30 sccm. After stabilization, an external voltage of 800 V was applied, and air plasma treatment was performed for 10 minutes to obtain a N2-NiFe-PBA catalyst.

[0059] Embodiment 6:

[0060] (a) Preparation of NiFe-PBA

[0061] Prepared according to the method and conditions of step (a) in Example 5.

[0062] (b) Preparation of N2-NiFe-PBA

[0063] The NiFe-PBA precursor prepared in step (a) was placed in a gas plasma chamber, and the pressure in the chamber was maintained below 0.8 mbar under reduced pressure. N2 was introduced at a flow rate of 30 sccm. After stabilization, an external voltage of 600 V was applied. The air plasma treatment was performed for 10 minutes. The obtained sample was N2-NiFe-PBA-600.

[0064] Embodiment 7:

[0065] (a) Preparation of NiFe-PBA

[0066] Prepared according to the method and conditions of step (a) in Example 5.

[0067] (b) Preparation of N2-NiFe-PBA

[0068] The NiFe-PBA precursor prepared in step (a) was placed in a gas plasma chamber, and the pressure in the chamber was maintained below 0.8 mbar under reduced pressure. N2 was introduced at a flow rate of 30 sccm. After stabilization, an external voltage of 700 V was applied. The air plasma treatment was performed for 10 minutes. The obtained sample was N2-NiFe-PBA-700.

[0069] Embodiment 8:

[0070] (a) Preparation of NiFe-PBA

[0071] Prepared according to the method and conditions of step (a) in Example 5.

[0072] (b) Preparation of N2-NiFe-PBA

[0073] The NiFe-PBA precursor prepared in step (a) was placed in a gas plasma chamber, and the pressure in the chamber was maintained below 0.8 mbar under reduced pressure. N2 was introduced at a flow rate of 30 sccm. After stabilization, an external voltage of 900 V was applied. The air plasma treatment was performed for 10 minutes. The obtained sample was N2-NiFe-PBA-900.

[0074] Embodiment 9:

[0075] (a) Preparation of CoFe-PBA

[0076] Three pieces of 2×3cm 2 The nickel foam was ultrasonically treated with 1 mol / L hydrochloric acid solution, deionized water and ethanol for 30, 5 and 10 min, respectively, and dried at 50°C for 6 h; 0.4366 g Co(NO3)2·6H2O and 0.6617 g Na3C6H5O7·2H2O were dissolved in 50 mL deionized water to form a clear solution A; 0.3293 g K3[Fe(CN)6] was dissolved in 50 mL deionized water to form a solution B; under magnetic stirring, solution B was slowly added to solution A to form a mixed solution C at room temperature; the pretreated nickel foam was soaked in the mixed solution C for 24 h, washed with deionized water and ethanol for 3 times, respectively, and dried at 50°C overnight to obtain a CoFe-PBA precursor.

[0077] (b) Preparation of N2-CoFe-PBA

[0078] The CoFe-PBA precursor prepared in step (a) was placed in a gas plasma chamber, and the pressure in the chamber was maintained below 0.8 mbar by reducing the vacuum. N2 was introduced at a flow rate of 30 sccm. After stabilization, an external voltage of 800 V was applied, and air plasma treatment was performed for 10 minutes to obtain a N2-CoFe-PBA catalyst.

[0079] Embodiment 10:

[0080] (a) Preparation of CoFe-PBA

[0081] Prepared according to the method and conditions of step (a) in Example 9.

[0082] (b) Preparation of N2-CoFe-PBA

[0083] The CoFe-PBA precursor prepared in step (a) was placed in a gas plasma chamber, and the pressure in the chamber was maintained below 0.8 mbar under reduced pressure. N2 was introduced at a flow rate of 30 sccm. After stabilization, an external voltage of 600 V was applied, and air plasma treatment was performed for 10 minutes to obtain a N2-CoFe-PBA-600 catalyst.

[0084] Embodiment 11:

[0085] (a) Preparation of CoFe-PBA

[0086] Prepared according to the method and conditions of step (a) in Example 9.

[0087] (b) Preparation of N2-CoFe-PBA

[0088] The CoFe-PBA precursor prepared in step (a) was placed in a gas plasma chamber, and the pressure in the chamber was maintained below 0.8 mbar under reduced pressure. N2 was introduced at a flow rate of 30 sccm. After stabilization, an external voltage of 700 V was applied, and air plasma treatment was performed for 10 minutes to obtain a N2-CoFe-PBA-700 catalyst.

[0089] Embodiment 12:

[0090] (a) Preparation of CoFe-PBA

[0091] Prepared according to the method and conditions of step (a) in Example 9.

[0092] (b) Preparation of N2-CoFe-PBA

[0093] The CoFe-PBA precursor prepared in step (a) was placed in a gas plasma chamber, and the pressure in the chamber was maintained below 0.8 mbar under reduced pressure. N2 was introduced at a flow rate of 30 sccm. After stabilization, an external voltage of 900 V was applied, and air plasma treatment was performed for 10 minutes to obtain a N2-CoFe-PBA-900 catalyst.

[0094] Comparative Example 1:

[0095] Preparation of NiCoFe-PBA

[0096] Prepared according to the method and conditions of step (a) in Example 1.

[0097] Comparative Example 2:

[0098] Preparation of NiFe-PBA

[0099] Prepared according to the method and conditions of step (a) in Example 5.

[0100] Comparative Example 3:

[0101] Preparation of CoFe-PBA

[0102] Prepared according to the method and conditions of step (a) in Example 9;

[0103] Figure 1They are respectively the scanning electron microscope images of NiCoFe-PBA (A) obtained in Comparative Example 1, the N2-NiCoFe-PBA (B) obtained in Example 1, and the transmission electron microscope images of N2-NiCoFe-PBA (C) obtained in Example 1. It can be seen from the figure that the size of NiCoFe-PBA is about 200nm, and the NiCoFe-PBA nanocubes with clear corners and edges are evenly covered on the surface of nickel foam. After N2 plasma activation, N2-NiCoFe-PBA retains the nanocube morphology, but the surface becomes rougher than the NiCoFe-PBA precursor. The plasma-induced high-energy nitrogen radicals can cut the Fe-C bonds, Ni(Co)-N bonds, and C≡N bonds in the NiCoFe-PBA crystals, among which the bond energy of C≡N is stronger, so the CN vacancies are introduced into the NiCoFe-PBA lattice by the plasma. In addition, the interior of the cubes will be preferentially etched by the plasma because their structure is looser than the compact outer surface and the defect density is higher. Therefore, the transmission electron microscopy image of N2-NiCoFe-PBA shows that the cube presents a nanocage structure, in which a crystalline-amorphous heterostructure is formed along the diagonal of the N2-NiCoFe-PBA nanocage. Among them, the crystalline phase and the amorphous phase provide high conductivity and abundant unsaturated coordination sites, respectively, to achieve rapid electron transfer and provide abundant active sites.

[0104] Figure 2 XRD diagrams of NiCoFe-PBA obtained in Comparative Example 1 and N2-NiCoFe-PBA obtained in Example 1. NiCoFe-PBA exhibits a set of characteristic diffraction peaks of PBA without impurities, indicating that NiCoFe-PBA is a single-phase structure. By comparing with the standard card, it is found that the main components of the NiCoFe-PBA sample correspond to the relative positions of the absorption peaks of KNiFe(CN)6 and Co3[Fe(CN)6]2!10H2O, but the absolute positions have a slight shift. This is because the introduction of the third metal will cause a certain degree of lattice contraction. After N2 plasma treatment, the N2-NiCoFe-PBA nanocage has diffraction peaks in the same position, but the absorption peak intensity is reduced and the half-peak width is widened relative to the NiCoFe-PBA precursor. This is attributed to the introduction of amorphous defect structure by N2 plasma.

[0105] The following electrocatalytic performance tests all used a saturated Hg / HgO electrode as the reference electrode, a stone mill rod electrode as the counter electrode, a scan rate of 1 mV / s, and a compensation degree of 90%.

[0106] Figure 3 The catalysts NiCoFe-PBA, NiFe-PBA and CoFe-PBA obtained in Comparative Example 1, Comparative Example 2 and Comparative Example 3 were 1.0 mol L -1OER linear sweep voltammetry curve in KOH solution. It can be seen from the figure that NiCoFe-PBA catalyst has the lowest overpotential. This is because the synergistic effect between trimetallic catalysts is better than that between bimetallic catalysts. Therefore, NiCoFe-PBA catalyst has the lowest overpotential at 1.0 mol L -1 The OER electrocatalytic performance in KOH solution is the best.

[0107] Figure 4 The catalysts N2-NiCoFe-PBA, N2-NiCoFe-PBA-600, N2-NiCoFe-PBA-700 and N2-NiCoFe-PBA-900 obtained in Example 1, Example 2, Example 3 and Example 4 were heated to 1.0 mol L -1 Linear sweep voltammetry curve of OER in KOH solution. Figure 4 It can be seen that when the N2 plasma treatment voltage is 800V, the obtained catalyst has the best electrocatalytic performance, which proves that the different V CN It has a regulating effect on catalytic performance.

[0108] Figure 5 The catalysts N2-NiFe-PBA, N2-NiFe-PBA-600, N2-NiFe-PBA-700 and N2-NiFe-PBA-900 obtained in Example 5, Example 6, Example 7 and Example 8 were heated to 1.0 mol L -1 Linear sweep voltammogram of OER in KOH solution. Figure 5 It can be seen that when the N2 plasma treatment voltage is 800V, the obtained catalyst has the best electrocatalytic performance, which once again proves that different V CN It has a regulating effect on catalytic performance.

[0109] Figure 6 The catalysts N2-CoFe-PBA, N2-CoFe-PBA-600, N2-CoFe-PBA-700 and N2-CoFe-PBA-900 obtained in Example 9, Example 10, Example 11 and Example 12 were heated to 1.0 mol L -1 Linear sweep voltammogram of OER in KOH solution. Figure 6 It can be seen that when the N2 plasma treatment voltage is 800V, the obtained catalyst has the best electrocatalytic performance, which verifies the CN It has a regulating effect on catalytic performance.

[0110] From the above three sets of experimental results, it can be concluded that N2 plasma treatment at a voltage of 800V can obtain binary and ternary PBAs with the best OER catalytic performance.

[0111] Figure 7 The catalysts N2-NiCoFe-PBA, N2-NiFe-PBA, N2-CoFe-PBA, NiCoFe-PBA, NiFe-PBA, CoFe-PBA obtained in Example 1, Example 5, Example 9, Comparative Example 1, Comparative Example 2, and Comparative Example 3 were quenched at 1.0 mol L -1 Linear sweep voltammetry curves of OER in KOH. Figure 7 It can be seen at 100mAcm -2 When the overpotential (η 100 ) are 286 and 391 mV, respectively, which are much lower than the corresponding N2-NiFe-PBA (312 mV), N2-CoFe-PBA (305 mV) and NiFe-PBA (415 mV), CoFe-PBA (404 mV), respectively. The results show that the interaction between the three metal sites can significantly enhance the OER activity. In addition, the η100 values ​​of the three groups of N2-PBA catalysts are 99 to 117 mV smaller than the overpotential of the corresponding PBA precursors, indicating that N2 plasma treatment plays a key role in improving the OER activity of PBA.

[0112] Figure 8 The catalysts N2-NiCoFe-PBA and NiCoFe-PBA obtained in Example 1 and Comparative Example 1 were - 1 KOH + 0.5 mol L -1 Linear sweep voltammetry curve of OER in NaCl mixed solution. The figure shows that -1 KOH + 0.5 mol L -1 In NaCl mixed solution, N2-NiCoFe-PBA catalyst has better OER catalytic performance than NiCoFe-PBA precursor, reaching 100mAcm -2 The overpotential required at a current density of only 293 mV is much lower than the η of the NiCoFe-PBA precursor. 100 (405mV); and the η of N2-NiCoFe-PBA in alkaline simulated seawater 100 The value is similar to η in its alkaline solution 100 The value (286mV) is almost the same, indicating that V CN The introduction of greatly improved the chloride ion corrosion resistance of N2-NiCoFe-PBA.

[0113] Fig. 9 The catalysts N2-NiCoFe-PBA and NiCoFe-PBA obtained in Example 1 and Comparative Example 1 were- 1 Linear sweep voltammetry curve of OER in KOH + natural seawater mixed solution. Fig. 9 It can be seen that even in alkaline natural seawater solution, the catalyst N2-NiCoFe-PBA has a very superior catalytic performance, reaching 100 mA cm -2 The overpotential required is only 323 mV at a current density of 1.5 Å, which is significantly lower than the η of the NiCoFe-PBA precursor. 100 (434 mV), demonstrating that the catalyst has good alkaline seawater oxidation ability.

[0114] Fig.10 The catalyst N2-NiCoFe-PBA obtained in Example 1 was added at 1.0 mol L -1 Stepwise chronopotentiograph (a) and constant current chronopotentiograph (b) in KOH. Fig.10 It can be seen that at 1.0 mol L -1 After the stability test in KOH solution, the potential of the N2-NiCoFe-PBA catalyst remained stable, demonstrating its good durability in alkaline solution.

[0115] Fig.11 The catalysts N2-NiCoFe-PBA and NiCoFe-PBA obtained in Example 1 and Comparative Example 1 were quenched in 1.0 mol L - 1 KOH + 0.5 mol L -1 The constant current chronopotentiometry curve in NaCl mixed solution. It can be seen that at 1.0 mol L -1 In KOH solution, after more than 20 hours of stability test, the potential of N2-NiCoFe-PBA catalyst hardly increased, while the potential of NiCoFe-PBA increased significantly, which proved that V CN The introduction of makes N2-NiCoFe-PBA much more stable than NiCoFe-PBA in alkaline simulated seawater.

[0116] Fig.12 The N2-NiCoFe-PBA (A and B) obtained in Example 1 and the NiCoFe-PBA (C and D) obtained in Comparative Example 1 were heated to 1.0 mol L -1 KOH + 0.5 mol L -1 SEM images after 24h stability test in NaCl mixed solution. As can be seen from Figures (A and B), after the stability test, NiCoFe-PBA evolved into a coating with many obvious cracks due to the [Fe(CN)6] 4-The NiCoFe-PBA nanocube skeletons collapsed and connected together to form nanosheets. CN It can effectively inhibit the [Fe(CN)6] 4- Therefore, Figures (C and D) show that the cubic framework of the N2-NiCoFe-PBA catalyst is retained after the stability test, presenting a dense film composed of tightly packed hollow nanocages, which can provide more active sites and fast mass / electron transfer to accelerate the OER kinetics.

[0117] Fig.13 The N2-NiCoFe-PBA obtained in Example 1 was added to 1.0 mol L -1 Constant current chronopotentiometry curves in KOH+natural seawater (a), N2-NiCoFe-PBA obtained in Example 1 and NiCoFe-PBA obtained in Comparative Example 1 at 1.0 mol L -1 KOH+2molL -1 The constant current chronopotentiometry curve in NaCl mixed solution (b). As can be seen from Figure a, in alkaline natural seawater, the N2-NiCoFe-PBA catalyst still exhibits very excellent electrocatalytic stability. After 12 hours of testing, its potential increase is negligible, indicating that the FeOOH layer formed on its surface and V CN They can respectively block and repel chloride ions from reaching the catalytic interface, thus improving the catalyst's resistance to chloride ion corrosion. As can be seen from Figure b, even in an alkaline solution with a high salt concentration, the N2-NiCoFe-PBA catalyst can -2 The results of the two groups of stability tests show that the formation of FeOOH layer and V CN The introduction of has a significant effect on improving the catalyst's resistance to chloride ion corrosion.

Claims

1. A Prussian blue-based oxygen evolution electrocatalyst rich in cyanide vacancies; characterized in that The electrocatalyst is based on nickel foam, and the nickel-cobalt-iron Prussian blue cube is an amorphous phase rich in cyanide vacancies along the diagonal, while the edge of the cube is a crystalline nickel-cobalt-iron Prussian blue phase; during the preparation process of the electrocatalyst, the concentration of cyanide vacancies is adjusted by controlling the nitrogen plasma voltage, and during the oxygen evolution process, the surface of the nickel-cobalt-iron Prussian blue is in situ converted into a NiCoFeOOH active phase; the cyanide vacancies are denoted as V CN ; Nickel-cobalt-iron Prussian blue is denoted as NiCoFe-PBA; Prussian blue-based oxygen evolution electrocatalyst rich in cyanide vacancies is denoted as N2-NiCoFe-PBA; The preparation method of the electrocatalyst is characterized by comprising the following specific steps: (a) Preparation of NiCoFe-PBA Three pieces of 2×3cm 2 The nickel foam was ultrasonically treated with 1 mol / L hydrochloric acid solution, deionized water and ethanol for 30, 5 and 10 min respectively, and dried at 50°C for 6 h; 0.2181 g Ni(NO3)2·6H2O, 0.2183 g Co(NO3)2·6H2O and 0.6617 g Na3C6H5O7·2H2O were dissolved in 50 mL deionized water to form a clear solution A; 0.3293 g K3[Fe(CN)6] was dissolved in 50 mL deionized water to form a solution B; under magnetic stirring, solution B was slowly added to solution A to form a mixed solution C at room temperature; the pretreated nickel foam was soaked in the mixed solution C for 24 h, washed with deionized water and ethanol for 3 times respectively, and dried at 50°C overnight to obtain NiCoFe-PBA precursor; (b) Preparation of N2-NiCoFe-PBA The NiCoFe-PBA precursor prepared in step (a) is placed in a gas plasma chamber, the pressure in the chamber is kept below 0.8 mbar by reducing the pressure, N2 is introduced at a flow rate of 30 sccm, and after stabilization, an external voltage of 600 V to 900 V is applied, and air plasma treatment is performed for 5 to 40 minutes to obtain a N2-NiCoFe-PBA catalyst; The prepared NiCoFe-PBA precursor is uniformly distributed nanocubes with a size of ~200nm and clear corners and edges; after N2 plasma activation, N2-NiCoFe-PBA retains the nanocube morphology well, but its surface becomes rougher than the NiCoFe-PBA precursor, and the cubes are transformed into an amorphous phase rich in cyanide vacancies along the diagonal, while the edges of the cubes are crystalline NiCoFe-PBA phase; during the OER process, a FeOOH protective layer is formed on the surface of N2-NiCoFe-PBA, which can effectively inhibit the corrosion of the catalyst and improve its stability and durability.

2. A Prussian blue-based oxygen evolution electrocatalyst rich in cyanide vacancies according to claim 1, characterized in that The catalyst is used for anodic oxygen evolution reaction in alkaline simulated seawater and alkaline natural seawater.