High-flexibility core-shell structure conductive magnetic fiber and preparation method and application thereof

The coaxial wet spinning method for flexible core-shell structured conductive magnetic fibers addresses scalability and cost issues, achieving high flexibility, conductivity, and adjustable magnetism, suitable for wearable electronics and communication technology.

CN119082933AActive Publication Date: 2024-12-06ZJU HANGZHOU GLOBAL SCI & TECH INNOVATION CENT

Patent Information

Application Number
CN202411313292.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-20
Publication Date
2024-12-06
Estimated Expiration
2044-09-20

AI Technical Summary

Technical Problem

Existing methods for producing flexible conductive or magnetic fibers are cumbersome, costly, and difficult to scale, often requiring multiple steps and organic solvents, leading to poor flexibility and stability due to the use of rigid fillers or hard magnetic powders, which also degrade tensile properties under high load.

Method used

A method for preparing highly flexible core-shell structured conductive magnetic fibers using coaxial wet spinning, involving the preparation of magnetic continuous and conductive metal dispersed phase solutions, with controlled injection rates and a rotating coagulation bath to form fibers with high flexibility, conductivity, and adjustable magnetism, utilizing thermoplastic polyurethane, polymer dispersants, and specific liquid metals like gallium-indium-tin alloys.

Benefits of technology

The method enables simple, low-cost, large-scale continuous production of fibers with high flexibility, strong conductivity, and adjustable magnetism, suitable for wearable electronics and communication technology, with improved tensile properties and electromagnetic shielding performance.

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119082933A_ABST
    Figure CN119082933A_ABST
Patent Text Reader

Abstract

The invention discloses a high-flexibility core-shell structure conductive magnetic fiber and a preparation method and application thereof, and belongs to the technical field of high polymer materials and conductive materials. According to the method, the conductive magnetic fiber with the core-shell structure can be continuously prepared on a large scale without multiple operation steps, the defects that the steps of synthesizing the core-shell structure through a multi-step method are tedious, experimental consumable reagents are wasted, and time is wasted are overcome, and the method has the advantages of being simple, efficient, low in cost and capable of saving time. The prepared high-flexibility core-shell structure conductive magnetic fiber has the characteristics of high flexibility, strong conductivity and adjustable magnetism, shows hydrophobicity and good electromagnetic shielding performance, and has good application prospects in the fields of sensing detection, electromagnetic shielding and the like.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention relates to the technical field of polymer materials and conductive materials, and specifically relates to a highly flexible core-shell structure conductive magnetic fiber and a preparation method and application thereof. Background Art

[0002] With the development of wearable electronic devices and communication technology in various fields, on the one hand, it has brought great convenience to human life, but on the other hand, it has also caused a series of problems such as serious electromagnetic radiation and interference. Therefore, people have begun to pay more and more attention to the research of protective fiber fabrics. In order to obtain satisfactory conductivity or magnetism, traditional protective fiber fabrics require a high concentration of rigid conductive or magnetic fillers, which usually leads to poor flexibility and stability of the fiber.

[0003] Recently, the emerging flexible liquid metal (LM) has attracted extensive attention from researchers due to its excellent fluidity and conductivity. However, due to the large surface tension of LM, it will increase the difficulty of processing in fiber structures. In addition, directly exposed liquid metal is easily oxidized and erased by external forces. Therefore, it is necessary to construct a reasonable stretchable liquid metal conductive fiber structure.

[0004] However, the current method for preparing such stretchable liquid metal conductive fibers is relatively cumbersome, requiring two or even more steps to couple the stretching material and the liquid material together. This type of method ([1]Angew. Chem., Int. Ed. 2013, 52,13453−13457.[2]Journal of Materials Research and Technology.2023.25.4728-4738.[3]Chemical Engineering Journal 10.1016 / j.cej.2021.129962.) is complex to operate and requires not only a large amount of organic solvents, but also a high-cost manufacturing process. It is not only time-consuming and reagent-intensive, but also cannot be prepared continuously, which limits its practical production and makes it difficult to further promote its application.

[0005] The preparation of conductive fibers based on coaxial wet spinning technology is a feasible strategy to solve the defects of the above-mentioned process. For example, the Chinese invention patent with publication number CN114703555A discloses a one-step molding batch preparation method of a core-shell structure liquid metal conductive fiber, which uses a shell layer syringe to extract a polyurethane solution and a core layer syringe to extract a gallium-based liquid metal; start spinning, first start the shell layer injection pump, the polyurethane solution is extruded through the injection pump and solidified through a coagulation bath; then start the core layer injection pump to ensure that the liquid metal is sealed and wrapped inside the polyurethane shell layer, and a core-shell structure liquid metal conductive fiber with a core layer of liquid metal and a shell layer of polyurethane is prepared. This invention overcomes the large surface tension of liquid metal, and the prepared liquid metal conductive fiber has excellent tensile properties and conductivity. For example, the Chinese invention patent with publication number CN111549396A provides a fiber wrapped with liquid metal and a preparation method thereof, firstly obtains a polymer fiber with a hollow structure, collects it through a conveyor belt and a turntable, and then injects liquid metal into the fiber cavity by injection to form a fiber wrapped with liquid metal. The fiber prepared by the invention has uniform structure, controllable size, good conductivity, and can be stretched and deformed.

[0006] However, the above processes mainly focus on the production and preparation of conductive fibers, while magnetic powder needs to be added in the manufacturing process of magnetic fibers. As a hard material, magnetic powder particles will deteriorate the tensile properties of the fiber after addition. This degradation is particularly obvious under high load rate conditions, thus affecting the normal use of subsequent magnetic fibers. In view of this, designing a simple, low-cost and large-scale continuous preparation method to prepare fibers with high flexibility, high conductivity and adjustable magnetism is of great significance to related fields such as wearable electronic devices and communication technology. Summary of the invention

[0007] In view of the above-mentioned defects of the prior art, in a first aspect of the present invention, a method for preparing a highly flexible core-shell structure conductive magnetic fiber with simple process, low cost and conducive to large-scale continuous production is provided, comprising the following steps: (1) Preparation of magnetic continuous phase solution: Thermoplastic polyurethane is dissolved in an organic solvent to obtain a polyurethane solution; a polymer dispersant is added to the polyurethane solution to form a uniform foam solution; magnetic powder is then added to the uniform foam solution and mixed to obtain a magnetic continuous phase solution; (2) Preparation of magnetic conductive metal dispersed phase solution: The liquid metal is treated with acid to remove the surface oxide layer, and then magnetic powder is added to the liquid metal, followed by ultrasonic dispersion and washing to obtain a magnetic conductive metal dispersed phase solution; (3) Preparation of highly flexible core-shell conductive magnetic fibers: A magnetic continuous phase solution and a magnetic conductive metal dispersed phase solution are used as the raw materials of the shell layer and the core layer respectively for coaxial spinning. The injection rate of the shell layer is controlled to be greater than that of the core layer, so that the core layer is squeezed and wrapped in the shell layer at the outlet of the coaxial spinning needle, and then continuously formed into a line in a rotating coagulation bath to obtain a highly flexible core-shell structured conductive magnetic fiber.

[0008] The organic solvent should have good solubility and be able to fully dissolve the polyurethane for easy processing and application. The polarity of the organic solvent should be close to the polarity of the polyurethane molecule to achieve effective dissolution. Common organic solvents for dissolving polyurethane include ketones, aromatic hydrocarbons, and amides, such as dimethylformamide, acetone, butanone, toluene, etc., which are all suitable types of selection for the present invention.

[0009] Preferably, in step (1), the organic solvent comprises at least one of dimethylformamide, acetone, butanone and toluene.

[0010] The polymer dispersant has an excellent dispersing effect and can effectively disperse the granular material into the solvent to form a uniform and stable dispersion system. In particular, in the present invention, the polymer dispersant represented by polyvinyl pyrrolidone, polyacrylic acid, and polyvinyl alcohol can not only promote the dispersion of magnetic powder, but also achieve high load through the foam structure formed by it. The dosage and molecular weight of the polymer dispersant are appropriately controlled within a suitable range. When its molecular weight is too low, it cannot play the role of the dispersant and cannot be used to adjust the load of the magnetic powder; when its molecular weight is too high, it is difficult to dissolve, which will affect its adsorption effect on the particle surface, thereby reducing the dispersion efficiency, or forming flocculation, which seriously affects the dispersion effect.

[0011] Preferably, in step (1), the polymer dispersant includes one of polyvinyl pyrrolidone, polyacrylic acid and polyvinyl alcohol.

[0012] Preferably, in step (1), the weight average molecular weight of the polymer dispersant is 1000-2000000.

[0013] Preferably, in step (1), the mass ratio of thermoplastic polyurethane to polymer dispersant is 10:1-10.

[0014] Preferably, in step (1), in the uniform foam solution, the concentration of the thermoplastic polyurethane is 1 wt.%-20 wt.%; and the concentration of the polymer dispersant is 1 wt.%-20 wt.%.

[0015] Generally, high loading rate magnetic powder will deteriorate the stretchability. In the prior art, the stretchability is about 350% without a magnetic shell. However, the process of the present invention can utilize the porous structure of the foam to make the fiber still have stretch resilience under the condition of hard magnetic powder, so that the fiber can reach the 350% stretchability index with a magnetic shell without obvious deterioration, and the magnetic properties can be adjusted by adding the proportion of magnetic powder.

[0016] Preferably, in step (1), the concentration of the magnetic powder in the magnetic continuous phase solution is 10 wt.%-70 wt.%.

[0017] Preferably, in step (1) and step (2), the magnetic powder comprises one of iron powder, ferrite powder and Ru-Fe-B powder.

[0018] Among liquid metals, gallium-indium-tin alloys or gallium-indium alloys have very low melting points, usually below room temperature, which means they can remain in liquid state at room temperature. The above alloys are materials with good biocompatibility and are suitable as raw materials for the production of wearable flexible electronic devices. Among them, the commercially available Ga68.5In21.5Sn10 and Ga75In25 (the symbol and number represent the type of element and mass fraction, respectively) have the advantages of cost-effectiveness and wide sources, and are particularly suitable liquid metal choices.

[0019] Preferably, in step (2), the liquid metal comprises gallium-indium-tin alloy or gallium-indium alloy.

[0020] Further preferably, the liquid metal includes gallium-indium-tin alloy Ga68.5In21.5Sn10 or gallium-indium alloy Ga75In25.

[0021] Preferably, in step (2), the ratio of the amount of magnetic powder to the amount of liquid metal is 1 wt.%-10 wt.%.

[0022] Preferably, in the step (3), during the coaxial spinning process, the injection rate of the magnetic continuous phase solution is 10-20 mL / h; and the injection rate of the magnetic conductive metal dispersed phase solution is 5-10 mL / h.

[0023] The overall fiber diameter of the highly flexible core-shell structured conductive magnetic fiber can be adjusted by changing the inner diameters of the two syringe needles to obtain fibers of different specifications to flexibly meet the needs of different applications.

[0024] Preferably, in step (3), the inner diameter of the needle for injecting the magnetic continuous phase solution is 0.3-3 mm; the inner diameter of the needle for injecting the magnetic conductive metal dispersed phase solution is 0.2-2 mm.

[0025] Preferably, in step (3), the speed of the rotating coagulation bath is 10-500 r / min.

[0026] In the second aspect of the present invention, a highly flexible core-shell structured conductive magnetic fiber with high flexibility, strong conductivity and adjustable magnetism is provided, which is prepared by the preparation method of the first aspect of the present invention.

[0027] In the third aspect of the present invention, there is provided an application of the highly flexible core-shell structure conductive magnetic fiber of the second aspect of the present invention, specifically, an application as a fiber material in sensing detection and electromagnetic shielding.

[0028] Preferably, the application includes the following steps: fixing the highly flexible core-shell structure conductive magnetic fiber at the finger joints, when the finger bending angle increases, the corresponding output voltage also increases, so that different gestures produce clear and repeatable signal patterns.

[0029] Further preferably, the length of the highly flexible core-shell structured conductive magnetic fiber is 3-6 cm.

[0030] Preferably, the application comprises the following steps: making the highly flexible core-shell structured conductive magnetic fiber into a fiber braid and using it for electromagnetic shielding.

[0031] Since magnetic powder is a hard material, as the magnetic powder loading rate increases, the extrusion of the wet coaxial spinning shell will become more and more difficult, resulting in discontinuous fiber preparation, which is the technical difficulty that the process of the present invention needs to solve. In the research and development stage, the inventor found that it is difficult to make the fiber have a high magnetic powder loading rate by simply mixing thermoplastic polyurethane, polymer dispersant, and magnetic powder together. Based on the above technical scheme, the design concept and principle of the present invention are that after adding the dispersant to form a uniform foam solution, a large amount of magnetic powder can be dispersed in the foam structure of the former, which promotes the realization of high load. Utilizing the difference in the injection rate of the core layer and the shell layer solution, the magnetic conductive metal dispersed phase solution and the magnetic continuous phase solution are squeezed and wrapped in the shell layer at the outlet of the coaxial spinning needle based on fluid mechanics. Since magnetic powder is added to the raw materials of the shell layer and the core layer in this process, there is a magnetic interaction force between the core layer magnetic powder and the shell layer magnetic powder. When prepared, the core layer is continuously formed into a line under the combined action of gravity, centrifugal force, and interaction force with the shell layer magnetic powder in the rotating coagulation bath device. In this way, the micro-particle structure of the magnetic powder is used to adjust the surface tension of the liquid metal so that the core layer liquid can be continuously extruded, and the polymer dispersant is combined to adjust the loading rate of the core layer magnetic powder, adjust the core-shell structure in size, and adjust the magnetic properties of the conductive fiber, so that the preparation method has the characteristics of being simple, efficient, and capable of large-scale continuous preparation.

[0032] A large amount of uniform foam solution can be formed by a simple mixing method. For example, in actual operation, a polymer dispersant is added in small amounts several times, and then stirred at room temperature to achieve the target effect, and then the target total amount of magnetic powder is added in small amounts several times, and it is dispersed in the foam by mechanical stirring. Those skilled in the art can also adopt other mixing methods according to actual conditions to achieve the preparation of uniform foam solution and dispersion of magnetic powder. The rotating coagulation bath device is a simple coagulation bath device that can rotate clockwise or counterclockwise in the longitudinal axis (relative to the horizontal axis), and contains a coagulation bath, such as water. Compared with the prior art that uses a stretching roller structure to make the core layer change in volume under stretching to form a continuous conductive medium, this method can be continuously formed into a line under the influence of the above-mentioned force, and the liquid metal of the core layer has good continuity without stretching. Therefore, the fiber produced by this process can be directly temporarily stored in the coagulation bath without the use of a stretching roller, and the site utilization rate is higher.

[0033] Compared with the prior art, the present invention has the following advantages and beneficial effects: The present invention provides a method for preparing highly flexible core-shell structured conductive magnetic fibers, which can continuously prepare conductive magnetic fibers with core-shell structures in large quantities without multiple operation steps, avoiding the shortcomings of cumbersome steps of synthesizing core-shell structures by a multi-step method, waste of experimental consumables and reagents, and waste of time. The method has the advantages of being simple, efficient, low-cost, and time-saving.

[0034] The present invention provides a highly flexible core-shell structured conductive magnetic fiber, which has the characteristics of high flexibility, strong conductivity, adjustable magnetism, and exhibits hydrophobicity and good electromagnetic shielding performance.

[0035] The present invention provides an application of a highly flexible core-shell structured conductive magnetic fiber, which has good application prospects in the fields of sensing detection, electromagnetic shielding, etc. BRIEF DESCRIPTION OF THE DRAWINGS

[0036] Figure 1 Schematic diagram of the process of preparing highly flexible core-shell structured conductive magnetic fibers by coaxial wet spinning; Figure 2 The optical photographs of the highly flexible core-shell structure conductive magnetic fiber prepared in Example 1; wherein Figure (a) is an optical photograph of the fiber, and Figure (b) is an optical photograph of the continuously prepared fiber with a length of nearly 2 m; Figure 3 The scanning electron microscope (SEM) image and element scanning image of the cross section of the highly flexible core-shell structure conductive magnetic fiber prepared in Example 1; Figure 4 This is a stretching picture of the highly flexible core-shell structure conductive magnetic fiber prepared in Example 1; Figure 5 is the magnetic property (magnetichysteresis, HM) curve of the highly flexible core-shell structure conductive magnetic fiber prepared in Example 1-3; Figure 6 The conductivity picture of the highly flexible core-shell structure conductive magnetic fiber prepared in Example 1; wherein (a)-(d) correspond to blue, green, yellow and white LED bulbs respectively; Figure 7 This is a picture of the real-time output electrical signal of the highly flexible core-shell structure conductive magnetic fiber prepared in Example 1 under different gesture changes in application; Figure 8 The contact angle of the highly flexible core-shell structure conductive magnetic fiber prepared in Example 1; Fig. 9 The electromagnetic shielding performance of the highly flexible core-shell structured conductive magnetic fiber prepared in Example 1. DETAILED DESCRIPTION

[0037] The present invention is further described below by way of examples, but the present invention is not limited to the scope of the examples. The experimental methods in the following examples without specifying specific conditions are carried out according to conventional methods and conditions, or selected according to the product specifications.

[0038] Example 1 The preparation method of highly flexible core-shell structure conductive magnetic fiber comprises the following steps: (1) Preparation of magnetic continuous phase solution: 2 g of thermoplastic polyurethane was weighed and put into 20 mL of N,N-dimethylformamide solution, heated and stirred at 60 °C for 12 h, and then cooled at room temperature to completely dissolve the thermoplastic polyurethane to obtain a polyurethane solution; then 0.5 g of polyvinyl pyrrolidone (Mw: 1300000) powder was added to the polyurethane solution and mechanically stirred for 1 h to form a uniform foam solution; then 1.2 g of rubidium iron boron powder was added in batches, ultrasonically dispersed, and then washed with deionized water to obtain a magnetic continuous phase solution; (2) Preparation of magnetic conductive metal dispersed phase solution: Gallium indium tin alloy (Ga68.5In21.5Sn10) is placed in dilute hydrochloric acid and dispersed by ultrasound to remove the insulating oxide layer on its surface, then 5 wt.% of rubidium iron boron powder is added, and after ultrasonic dispersion, it is left to stand for a period of time and then washed with deionized water to obtain a magnetic conductive metal dispersed phase solution; (3) Preparation of highly flexible core-shell conductive magnetic fibers: like Figure 1As shown, the magnetic continuous phase solution and the magnetic conductive metal dispersed phase solution are used as the raw materials of the shell layer and the core layer in turn, and are loaded into the syringe of the coaxial wet spinning device respectively. The syringes are connected to the inner and outer phase ports of the coaxial spinning needle respectively, and two propellers are used to propel the shell layer syringe and the core layer syringe respectively, and the injection rate of the shell layer is controlled to be 15 mL / h, and the injection rate of the core layer is controlled to be 8 mL / h; deionized water is used as a coagulation bath, and the magnetic conductive metal dispersed phase solution and the magnetic continuous phase solution are used to extrude and wrap the core layer in the shell layer at the outlet of the coaxial spinning needle through fluid mechanics by utilizing the different injection rates of the two propellers. The core layer is continuously formed into a line in the rotating coagulation bath device under the combined action of gravity, centrifugal force and interaction force with the shell layer magnetic powder, so as to obtain a highly flexible core-shell structured conductive magnetic fiber.

[0039] Optical photos of highly flexible core-shell conductive magnetic fibers Figure 2 As shown. Figure (a) is an optical photograph of the fiber, and Figure (b) is an optical photograph of a fiber with a length of nearly 2 m prepared continuously. This method produces the finished product required by the design.

[0040] The cross section of the highly flexible core-shell conductive magnetic fiber was characterized by SEM and element scanning. Figure 3 shown. Figure 3 It was shown that the shell layer of the highly flexible core-shell structured conductive magnetic fiber had a porous structure, proving that the target structure was formed by a uniform foam solution in the process, which helped to prevent the performance degradation of magnetic particles while taking into account stretchability.

[0041] This example studies the tensile properties of the prepared highly flexible core-shell conductive magnetic fiber. Figure 4 As shown, a 2 cm long fiber is fixed at one end and the other end is mechanically stretched to its maximum length. The original 2 cm length of the fiber can be stretched to 7 cm, with a stretching rate of up to 350%.

[0042] A 1 cm long highly flexible core-shell conductive magnetic fiber was placed in a superconducting quantum interference device for testing at 300 K. The magnetic property curve is shown in Figure 2. Figure 5 As shown. At 2000 Oe, the saturation magnetization intensity of the fiber can reach 0.25 emu. Combined with the test results of Examples 2 and 3 below, it is shown that the magnetic adjustability of the highly flexible core-shell structure conductive magnetic fiber can be easily achieved by adjusting the amount of magnetic powder added.

[0043] The resistance of the highly flexible core-shell conductive magnetic fiber was tested using a digital multimeter, and the resistance value was 6.1 Ω. Figure 6As shown in the figure, an external voltage (1.8-3 V) and 8 cm conductive fiber are connected in series with blue, green, yellow and white LED bulbs respectively. When the external voltage is turned on, the corresponding LED bulb can be lit. When the voltage is turned off, the LED bulb goes out, proving that the conductive fiber has good conductivity.

[0044] Example 2 The preparation method of this embodiment is basically the same as that of embodiment 1, except that the amount of rubidium iron boron powder added in this embodiment is 1.0 g. The magnetic property curve is tested by the same method as above, and the results are as follows: Figure 5 The magnetic properties of the highly flexible core-shell structure conductive magnetic fiber of this embodiment are measured at 300 K, and the saturation magnetization intensity at 20000 Oe is 0.21emu.

[0045] Example 3 The preparation method of this embodiment is basically the same as that of embodiment 1, except that the amount of rubidium iron boron powder added in this embodiment is 0.8 g. The magnetic property curve is tested by the same method as above, and the results are as follows: Figure 5 The magnetic properties of the highly flexible core-shell structure conductive magnetic fiber of this embodiment are measured at 300 K, and the saturation magnetization intensity at 20000 Oe is 0.15emu.

[0046] Example 4 In this embodiment, the highly flexible core-shell conductive magnetic fiber prepared in Example 1 is applied to sensing detection. Figure 7 As shown, five highly flexible core-shell structured conductive magnetic fibers are fixed at the five finger joints. When the finger bending angle increases, the corresponding output voltage also increases. Each gesture movement can produce a clear and repeatable signal pattern.

[0047] Example 5 In this embodiment, the highly flexible core-shell structure conductive magnetic fiber prepared in Example 1 is further woven into a fabric through warp and weft threads, and the hydrophilicity and hydrophobicity of the fabric are measured in a contact angle measuring instrument. Figure 8 As shown in Figure 2, according to the contact angle results, it is proved that the fabric exhibits hydrophobic properties. The fabric is then cut into 10×10 mm 2 The electromagnetic shielding performance of the fabric was tested using the N5244A vector network analyzer produced by Agilent Technologies, USA. The waveguide method was used, and the test frequency band was 8.2-12.4 GHz (X band). The results are as follows: Fig. 9 As shown. The magnetic shielding effectiveness is 30.1 dB through testing and calculation. The above results show that the conductive fiber exhibits hydrophobicity and electromagnetic shielding performance in application.

[0048] Example 6 The preparation method of highly flexible core-shell structure conductive magnetic fiber comprises the following steps: (1) Preparation of magnetic continuous phase solution: Thermoplastic polyurethane (concentration: 1 wt.%) was placed in acetone, heated and stirred at 60 °C for 12 h, and then cooled at room temperature to completely dissolve the thermoplastic polyurethane to obtain a polyurethane solution; polyacrylic acid (Mw: 2000000; concentration: 1 wt.%) powder was then added to the polyurethane solution and mechanically stirred for 1 h to form a uniform foam solution, and the mass ratio of thermoplastic polyurethane to polyacrylic acid was 10:1; ferrite powder (concentration: 10 wt.%) was then added in batches, ultrasonically dispersed, and then washed with deionized water to obtain a magnetic continuous phase solution; (2) Preparation of magnetic conductive metal dispersed phase solution: Gallium-indium alloy (Ga75In25) is placed in dilute hydrochloric acid and dispersed by ultrasound to remove the insulating oxide layer on its surface, and then ferrite powder with a mass of 1 wt.% of gallium-indium alloy is added, and after ultrasonic dispersion, it is left to stand for a period of time and then washed with deionized water to obtain a magnetic conductive metal dispersed phase solution; (3) Preparation of highly flexible core-shell conductive magnetic fibers: The magnetic continuous phase solution and the magnetic conductive metal dispersed phase solution are used as the raw materials of the shell layer and the core layer respectively, and are loaded into the syringes of the coaxial wet spinning device respectively. The syringes are connected to the inner and outer phase ports of the coaxial spinning needle respectively, and two propellers are used to propel the shell layer syringe and the core layer syringe respectively. The injection rate of the shell layer is controlled to be 10 mL / h, and the injection rate of the core layer is controlled to be 5 mL / h. Deionized water is used as the coagulation bath. By utilizing the different injection rates of the two propellers, the magnetic conductive metal dispersed phase solution and the magnetic continuous phase solution extrude and wrap the core layer in the shell layer at the outlet of the coaxial spinning needle through fluid mechanics. The core layer is continuously formed into a line in the rotating coagulation bath device under the combined action of gravity, centrifugal force and interaction force with the shell layer magnetic powder, so as to obtain a highly flexible core-shell structured conductive magnetic fiber.

[0049] Example 7 The preparation method of highly flexible core-shell structure conductive magnetic fiber comprises the following steps: (1) Preparation of magnetic continuous phase solution: Thermoplastic polyurethane (concentration: 20 wt.%) was placed in toluene, heated and stirred at 60 °C for 12 h, and then cooled at room temperature to completely dissolve the thermoplastic polyurethane to obtain a polyurethane solution; polyvinyl alcohol (Mw: 1000; concentration: 20 wt.%) powder was then added to the polyurethane solution and mechanically stirred for 1 h to form a uniform foam solution, and the mass ratio of thermoplastic polyurethane to polyvinyl alcohol was 1:1; ferrite powder (concentration: 70 wt.%) was then added in batches, ultrasonically dispersed, and then washed with deionized water to obtain a magnetic continuous phase solution; (2) Preparation of magnetic conductive metal dispersed phase solution: Gallium indium tin alloy (Ga68.5In21.5Sn10) is placed in dilute hydrochloric acid and dispersed by ultrasound to remove the insulating oxide layer on its surface, then ferrite powder with a mass of 10wt.% of gallium indium tin alloy is added, and after ultrasonic dispersion, it is left to stand for a period of time and then washed with deionized water to obtain a magnetic conductive metal dispersed phase solution; (3) Preparation of highly flexible core-shell conductive magnetic fibers: The magnetic continuous phase solution and the magnetic conductive metal dispersed phase solution are used as the raw materials of the shell layer and the core layer respectively, and are loaded into the syringes of the coaxial wet spinning device respectively. The syringes are connected to the inner and outer phase ports of the coaxial spinning needle respectively, and two propellers are used to propel the shell layer syringe and the core layer syringe respectively. The injection rate of the shell layer is controlled to be 10 mL / h, and the injection rate of the core layer is controlled to be 5 mL / h. Deionized water is used as the coagulation bath. By utilizing the different injection rates of the two propellers, the magnetic conductive metal dispersed phase solution and the magnetic continuous phase solution extrude and wrap the core layer in the shell layer at the outlet of the coaxial spinning needle through fluid mechanics. The core layer is continuously formed into a line in the rotating coagulation bath device under the combined action of gravity, centrifugal force and interaction force with the shell layer magnetic powder, so as to obtain a highly flexible core-shell structured conductive magnetic fiber.

[0050] Example 8 The preparation method of highly flexible core-shell structure conductive magnetic fiber comprises the following steps: (1) Preparation of magnetic continuous phase solution: Thermoplastic polyurethane (concentration: 10 wt.%) was placed in butanone, heated and stirred at 60 °C for 12 h, and then cooled at room temperature to completely dissolve the thermoplastic polyurethane to obtain a polyurethane solution; polyvinyl pyrrolidone (Mw: 40000; concentration: 10 wt.%) powder was then added to the polyurethane solution and mechanically stirred for 1 h to form a uniform foam solution, and the mass ratio of thermoplastic polyurethane to polyvinyl pyrrolidone was 5:1; iron powder (concentration: 40 wt.%) was then added in batches, ultrasonically dispersed, and then washed with deionized water to obtain a magnetic continuous phase solution; (2) Preparation of magnetic conductive metal dispersed phase solution: Gallium indium tin alloy (Ga68.5In21.5Sn10) is placed in dilute hydrochloric acid and dispersed by ultrasound to remove the insulating oxide layer on its surface, then iron powder with a mass of 5wt.% of the gallium indium tin alloy is added, and after ultrasonic dispersion, it is left to stand for a period of time and then washed with deionized water to obtain a magnetic conductive metal dispersed phase solution; (3) Preparation of highly flexible core-shell conductive magnetic fibers: The magnetic continuous phase solution and the magnetic conductive metal dispersed phase solution were used as the raw materials of the shell layer and the core layer respectively, and were loaded into the syringes of the coaxial wet spinning device respectively. The syringes were connected to the inner and outer phase ports of the coaxial spinning needle respectively, and two propellers were used to propel the shell layer syringe and the core layer syringe respectively. The injection rate of the shell layer was controlled to be 20 mL / h, and the injection rate of the core layer was controlled to be 10 mL / h. Deionized water was used as the coagulation bath, and the magnetic conductive metal dispersed phase solution and the magnetic continuous phase solution squeezed and wrapped the core layer in the shell layer at the outlet of the coaxial spinning needle through fluid mechanics by utilizing the different injection rates of the two propellers. The core layer was continuously formed into a line in the rotating coagulation bath device under the combined action of gravity, centrifugal force and interaction force with the shell layer magnetic powder, so as to obtain a highly flexible core-shell structured conductive magnetic fiber.

[0051] In summary, in the preparation method of the present invention, a uniform foam solution is formed by adding a dispersant, and then the magnetic powder is added, so that a large amount of magnetic powder is dispersed in the foam structure of the former, which promotes the realization of high load, and the porous structure of the shell formed by the foam structure is used to maintain the tensile properties of the fiber, and prevent the magnetic powder from deteriorating the performance. The present invention uses the difference in injection rates of the two propellers to make the magnetic conductive metal dispersed phase solution and the magnetic continuous phase solution squeeze and wrap the core layer in the shell layer at the outlet of the coaxial spinning needle based on fluid mechanics. Since magnetic powder is added to the raw materials of the shell layer and the core layer in this process, there is a magnetic interaction force between the core layer magnetic powder and the shell layer magnetic powder. When prepared in this way, the core layer is continuously formed into a line under the combined action of gravity, centrifugal force and interaction force with the shell layer magnetic powder in the rotating coagulation bath device. In this way, the micro-particle structure of the magnetic powder is used to adjust the surface tension of the liquid metal so that the core layer liquid can be continuously extruded, and the polymer dispersant is combined to adjust the loading rate of the core layer magnetic powder, adjust the core-shell structure in size, and adjust the magnetic properties of the conductive fiber, so that the preparation method has the advantages of being simple, efficient, and capable of large-scale continuous preparation.

[0052] The highly flexible core-shell structure conductive magnetic fiber prepared by this process has adjustable core-shell part size, adjustable overall fiber diameter, and adjustable magnetism. The conductive fiber has continuous excellent conductivity, and can make LED bulbs of different colors light up using a relatively low voltage (1-3 V). The conductive fiber is also hydrophobic and exhibits electromagnetic shielding performance, with an electromagnetic shielding efficiency of up to 30.1 dB in the 8.2-12.4 GHz X-band frequency; when used for sensing detection, the real-time output electrical signal of the power-down is clear and unambiguous when different gestures change, and has broad application prospects.

[0053] The preferred specific embodiments of the present invention are described in detail above. It should be understood that a person skilled in the art can make many modifications and changes based on the concept of the present invention without creative work. Therefore, any technical solution that can be obtained by a person skilled in the art through logical analysis, reasoning or limited experiments based on the concept of the present invention on the basis of the prior art should be within the scope of protection determined by the claims.

Claims

1. A method for preparing a highly flexible core-shell structured conductive magnetic fiber, characterized in that: The steps include: (1) Preparation of magnetic continuous phase solution: Thermoplastic polyurethane is dissolved in an organic solvent to obtain a polyurethane solution; a polymer dispersant is added to the polyurethane solution to form a uniform foam solution; magnetic powder is then added to the uniform foam solution and mixed to obtain a magnetic continuous phase solution; (2) Preparation of magnetic conductive metal dispersed phase solution: The liquid metal is treated with acid to remove the surface oxide layer, and then magnetic powder is added to the liquid metal, followed by ultrasonic dispersion and washing to obtain a magnetic conductive metal dispersed phase solution; (3) Preparation of highly flexible core-shell conductive magnetic fibers: A magnetic continuous phase solution and a magnetic conductive metal dispersed phase solution are used as the raw materials of the shell layer and the core layer respectively for coaxial spinning. The injection rate of the shell layer is controlled to be greater than that of the core layer, so that the core layer is squeezed and wrapped in the shell layer at the outlet of the coaxial spinning needle, and then continuously formed into a line in a rotating coagulation bath to obtain a highly flexible core-shell structured conductive magnetic fiber.

2. The method for preparing the highly flexible core-shell structure conductive magnetic fiber according to claim 1, characterized in that: In the step (1), the organic solvent includes at least one of dimethylformamide, acetone, butanone, and toluene.

3. The method for preparing the highly flexible core-shell structure conductive magnetic fiber according to claim 1, characterized in that: In the step (1), the polymer dispersant includes one of polyvinyl pyrrolidone, polyacrylic acid, and polyvinyl alcohol; the weight average molecular weight of the polymer dispersant is 1000-2000000; and the mass ratio of thermoplastic polyurethane to the polymer dispersant is 10:1-10.

4. The method for preparing the highly flexible core-shell structure conductive magnetic fiber according to claim 1, characterized in that: In the step (1), in the uniform foam solution, the concentration of thermoplastic polyurethane is 1 wt.%-20 wt.%; the concentration of polymer dispersant is 1 wt.%-20 wt.%; and the concentration of magnetic powder in the magnetic continuous phase solution is 10 wt.%-70 wt.%.

5. The method for preparing the highly flexible core-shell structure conductive magnetic fiber according to claim 1, characterized in that: In the step (2), the liquid metal includes gallium-indium-tin alloy or gallium-indium alloy; the proportion of the magnetic powder used in the liquid metal is 1 wt.%-10 wt.%.

6. The method for preparing the highly flexible core-shell structure conductive magnetic fiber according to claim 1, characterized in that: In the step (3), during the coaxial spinning process, the injection rate of the magnetic continuous phase solution is 10-20 mL / h; the injection rate of the magnetic conductive metal dispersed phase solution is 5-10 mL / h; the inner diameter of the needle for injecting the magnetic continuous phase solution is 0.3-3 mm; the inner diameter of the needle for injecting the magnetic conductive metal dispersed phase solution is 0.2-2 mm; and the speed of the rotating coagulation bath is 10-500 r / min.

7. A highly flexible core-shell structure conductive magnetic fiber, characterized in that: The method is prepared by the preparation method according to any one of claims 1 to 6.

8. An application of the highly flexible core-shell structured conductive magnetic fiber as claimed in claim 7, characterized in that: Application as fiber material in sensing detection and electromagnetic shielding.

9. The use of the highly flexible core-shell structured conductive magnetic fiber according to claim 8, characterized in that: The application includes the following steps: fixing highly flexible core-shell structure conductive magnetic fibers at the finger joints, and when the finger bending angle increases, the corresponding output voltage also increases, so that different gestures produce clear and repeatable signal patterns.

10. The use of the highly flexible core-shell structured conductive magnetic fiber according to claim 8, characterized in that: The application comprises the following steps: making the highly flexible core-shell structured conductive magnetic fiber into a fiber braid and using it for electromagnetic shielding.

Citation Information

Patent Citations

  • Fiber coated with liquid metal and preparation method thereof

    CN111549396A

  • One-step forming batch preparation method of liquid metal conductive fiber with core-shell structure

    CN114703555A

  • Preparation method of magnetic polyurethane elastic fiber

    CN109943907A

  • Magnetic fiber material and preparation method and application thereof

    CN111155197A

  • Conductive fiber with resistance insensitive to tensile strain and preparation method thereof

    CN116516521A

Cited By

  • Flexible electrode capable of adjusting detection position in real time