Preparation method of antibacterial hydrophobic textile and product thereof
By using sodium hydroxide solution and copper sulfate solution in textiles to embed copper ions and react with cetyl trimethoxysilane at high temperature to form copper oxide, the complex process and inorganic particles of hydrophobic textiles in the prior art are solved. The problem of easy shedding has achieved the dual functions of textile preparation with antibacterial and hydrophobic functions.
Patent Information
- Application Number
- CN202411193027.7
- Authority / Receiving Office
- CN · China
- Patent Type
- Applications(China)
- Current Assignee / Owner
- Filing Date
- 2024-08-28
- Publication Date
- 2024-12-06
AI Technical Summary
The existing hydrophobic textile preparation process is complex and the inorganic particles are prone to fall off, which cannot effectively achieve antibacterial and hydrophobic versatility.
The cotton fabric was immersed with a saturated copper ion solution of sodium hydroxide and copper sulfate solution, and then treated in a reducing agent solution, and reacted with cetyl trimethoxysilane to convert the copper ions into The cuprous oxide is cured inside the fiber to achieve antibacterial and hydrophobicity.
Through this method, copper ions are stably bound inside the fiber, and cuprous oxide is formed on the fiber surface, achieving the dual functions of antibacterial and hydrophobicity, simplifying the process flow and improving the durability of the material.
Smart Images

Figure CN119083153A_ABST
Abstract
Description
Technical Field
[0001] The invention belongs to the field of textile technology, and specifically relates to a preparation method of an antibacterial and hydrophobic textile and a product thereof. Background Art
[0002] Cotton fabric is a common textile material with the advantages of good air permeability, moisture absorption, warmth retention and biodegradability.
[0003] With the improvement of living standards, people's requirements for cotton fabrics are no longer limited to breathable moisture absorption, warmth and cold protection. Multifunctional textiles such as hydrophobic, antibacterial and self-cleaning are becoming more and more popular.
[0004] At present, the preparation of hydrophobic textiles is mostly achieved through two steps: first, silica, titanium dioxide, carbon nanotubes, etc. are used to construct a micro-nanoscale rough structure on the surface of the fabric, and then low-surface energy chemical reagents are used to further treat it; however, this process is complicated, and the inorganic particles are mostly attached to the surface of the fabric and are easy to fall off during use. Summary of the invention
[0005] The purpose of this section is to summarize some aspects of embodiments of the present invention and briefly introduce some preferred embodiments. Some simplifications or omissions may be made in this section and the specification abstract and the invention title of this application to avoid blurring the purpose of this section, the specification abstract and the invention title, and such simplifications or omissions cannot be used to limit the scope of the present invention.
[0006] In view of the above problems and the problems existing in the prior art, the present invention is proposed.
[0007] Therefore, the object of the present invention is to overcome the deficiencies in the prior art and provide a method for preparing an antibacterial and hydrophobic textile.
[0008] In order to solve the above technical problems, the present invention provides the following technical solutions: a method for preparing an antibacterial hydrophobic textile, comprising:
[0009] A sodium hydroxide solution and a copper sulfate solution are prepared respectively, and the copper sulfate solution is added to the sodium hydroxide solution under stirring to obtain a saturated copper ion solution of sodium hydroxide;
[0010] The dry cotton fabric is immersed in a saturated copper ion solution of sodium hydroxide at room temperature for 24 hours, the cotton fabric is taken out, the sodium hydroxide on the surface of the cotton fabric is washed off with clean water, and the cotton fabric is dried at room temperature to obtain a pretreated cotton fabric;
[0011] The pretreated cotton fabric is immersed in a reducing agent solution at room temperature to obtain a reducing agent-treated cotton fabric;
[0012] The cotton fabric treated with the reducing agent is mixed with hexadecyltrimethoxysilane, reacted at high temperature, washed with clean water, and dried to obtain the antibacterial and hydrophobic textile.
[0013] As a preferred embodiment of the preparation method of the present invention, the concentration of the sodium hydroxide solution is 15wt%.
[0014] As a preferred embodiment of the preparation method of the present invention, the concentration of the copper sulfate solution is 0.02 mol / L.
[0015] As a preferred embodiment of the preparation method of the present invention, the mixing volume ratio of the sodium hydroxide solution to the copper sulfate solution is 1:1.
[0016] As a preferred embodiment of the preparation method of the present invention, the dry cotton fabric is immersed in a saturated copper ion solution of sodium hydroxide at a bath ratio of 1:100.
[0017] As a preferred solution of the preparation method of the present invention, the reducing agent solution comprises one of a gallnut extract solution, a honeysuckle extract solution and a glucose solution, and the mass fraction thereof is 1% to 5%.
[0018] As a preferred embodiment of the preparation method of the present invention, the pretreated cotton fabric is immersed in a reducing agent solution, wherein the bath ratio is 1:50 and the immersion time is 10 to 60 minutes.
[0019] As a preferred embodiment of the preparation method of the present invention, the cotton fabric treated with the reducing agent is mixed with hexadecyltrimethoxysilane, wherein the mass volume ratio of the cotton fabric to the hexadecyltrimethoxysilane is 1:60 to 1:120 g / mL.
[0020] As a preferred embodiment of the preparation method of the present invention, the reaction is carried out at a high temperature, wherein the reaction temperature is 120 to 200° C. and the reaction time is 20 to 75 minutes.
[0021] Another object of the present invention is to overcome the deficiencies in the prior art and provide an antibacterial and hydrophobic textile prepared by a method for preparing the antibacterial and hydrophobic textile.
[0022] Beneficial effects of the present invention:
[0023] (1) The present invention provides a method for preparing an antibacterial and hydrophobic textile, which comprises immersing a cotton fabric in a saturated copper ion solution of sodium hydroxide, using the sodium hydroxide solution to break the cellulose hydrogen bond network, embedding the copper ions into the gaps between cellulose crystals, and coordinating with the exposed oxygen-containing polar functional groups (such as hydroxyl groups) on the cellulose chains, and then immersing the cotton fabric in a reducing agent, and then heat-treating the cotton fabric with hexadecyltrimethoxysilane, converting the copper ions embedded in the fiber into stable cuprous oxide in situ, and fixing the hexadecyltrimethoxysilane on the surface of the fabric, thereby obtaining a textile having both antibacterial and hydrophobic functions.
[0024] (2) The present invention utilizes sodium hydroxide to destroy cellulose chains, allowing copper ions to penetrate into the cotton fabric at the molecular level and coordinate with cellulose. A reducing agent is used to reduce the copper ions to cuprous oxide, thereby constructing a rough surface on the cotton fabric and imparting it with antibacterial properties.
[0025] (3) The hexadecyltrimethoxysilane of the present invention is both a hydrophobic modifier and a high-temperature reaction solvent, and the hydrophobic modification and the in-situ formation of cuprous oxide are completed in only one step, thereby shortening the process time. BRIEF DESCRIPTION OF THE DRAWINGS
[0026] In order to more clearly illustrate the technical solutions of the embodiments of the present invention, the following briefly introduces the drawings required for describing the embodiments. Obviously, the drawings described below are only some embodiments of the present invention. For ordinary technicians in this field, other drawings can be obtained based on these drawings without creative labor. Among them:
[0027] Figure 1 These are pictures of cotton fabrics of the embodiments of the present invention and comparative examples;
[0028] Figure 2 is the XRD diagram of Example 1 of the present invention;
[0029] Figure 3 The figure is a test result diagram of the hydrophobicity of the cotton fabric of the present invention;
[0030] Figure 4 This is a graph showing the antibacterial performance test results of the cotton fabric of the present invention. DETAILED DESCRIPTION
[0031] In order to make the above-mentioned objects, features and advantages of the present invention more obvious and easy to understand, the specific implementation methods of the present invention are described in detail below in conjunction with the embodiments of the specification.
[0032] In the following description, many specific details are set forth to facilitate a full understanding of the present invention, but the present invention may also be implemented in other ways different from those described herein, and those skilled in the art may make similar generalizations without violating the connotation of the present invention. Therefore, the present invention is not limited to the specific embodiments disclosed below.
[0033] Secondly, the term "one embodiment" or "embodiment" as used herein refers to a specific feature, structure, or characteristic that may be included in at least one implementation of the present invention. The term "in one embodiment" that appears in different places in this specification does not necessarily refer to the same embodiment, nor does it refer to a separate or selective embodiment that is mutually exclusive with other embodiments.
[0034] The gallnut extract in the present invention was purchased from Shaanxi New Horizon Biotechnology Co., Ltd.
[0035] Hexadecyltrimethoxysilane was purchased from Hubei Yamade Biopharmaceutical Co., Ltd.;
[0036] Honeysuckle extract was purchased from Shaanxi New Horizon Biotechnology Co., Ltd.;
[0037] The specific preparation process of the saturated copper ion solution of sodium hydroxide in the present invention is:
[0038] A sodium hydroxide solution with a concentration of 15 wt% and a copper sulfate solution with a concentration of 0.02 mol / L were prepared, and the copper sulfate solution was slowly added to the sodium hydroxide solution under vigorous stirring. A small amount of copper hydroxide precipitate was removed by suction filtration to obtain a saturated copper ion solution of sodium hydroxide, wherein the mixing volume ratio of the sodium hydroxide solution to the copper sulfate solution was 1:1.
[0039] Example 1
[0040] (1) Take a clean cotton fabric and immerse it in a saturated copper ion solution of sodium hydroxide for 24 hours, wash it with deionized water until it is neutral, dry it and set it aside;
[0041] (2) preparing a 2% by mass solution of the gallnut extract, and immersing the cotton fabric treated in step (1) in the gallnut extract solution for 20 minutes;
[0042] (3) Hexadecyltrimethoxysilane is measured at a mass volume ratio of cotton fabric to hexadecyltrimethoxysilane of 1:100, and the cotton fabric treated in step (2) is added to the hexadecyltrimethoxysilane, reacted at 180° C. for 40 minutes, and then taken out, washed with a surfactant and deionized water, and then dried.
[0043] Comparative Example 1-1
[0044] (1) Take a clean cotton fabric and immerse it in a saturated copper ion solution of sodium hydroxide for 24 hours, wash it with deionized water until it is neutral, dry it and set it aside;
[0045] (2) Hexadecyltrimethoxysilane is measured at a mass volume ratio of cotton fabric to hexadecyltrimethoxysilane of 1:100, and the cotton fabric treated in step (1) is added to the hexadecyltrimethoxysilane, reacted at 180° C. for 40 minutes, and then taken out, washed with a surfactant and deionized water, and then dried.
[0046] Comparative Example 1-2
[0047] (1) Prepare a 2% by mass solution of gallnut extract, and immerse a portion of clean cotton fabric in the gallnut extract solution for 20 min;
[0048] (2) Hexadecyltrimethoxysilane is measured at a mass volume ratio of cotton fabric to hexadecyltrimethoxysilane of 1:100, and the cotton fabric treated in step (1) is added to the hexadecyltrimethoxysilane, reacted at 180° C. for 40 minutes, and then taken out, washed with a surfactant and deionized water, and then dried.
[0049] Comparative Examples 1-3
[0050] (1) Take a clean cotton fabric and immerse it in a 0.02 mol / L copper sulfate solution for 24 h, wash it with deionized water until it becomes neutral, dry it, and set it aside;
[0051] (2) Hexadecyltrimethoxysilane is measured at a mass volume ratio of cotton fabric to hexadecyltrimethoxysilane of 1:100, and the cotton fabric treated in step (1) is added to the hexadecyltrimethoxysilane, reacted at 180° C. for 40 minutes, and then taken out, washed with a surfactant and deionized water, and then dried.
[0052] Comparative Examples 1-4
[0053] (1) Take a clean cotton fabric and immerse it in a saturated copper ion solution of sodium hydroxide for 24 hours, wash it with deionized water until it is neutral, dry it and set it aside;
[0054] (2) preparing a 2% by mass solution of the gallnut extract, and immersing the cotton fabric treated in step (1) in the gallnut extract solution for 20 minutes, then taking it out, washing it with deionized water, and drying it.
[0055] Example 2
[0056] (1) Take a clean cotton fabric and immerse it in a saturated copper ion solution of sodium hydroxide for 24 hours, wash it with deionized water until it is neutral, dry it and set it aside;
[0057] (2) preparing a 1% by mass solution of the gallnut extract, and immersing the cotton fabric treated in step (1) in the gallnut extract solution for 10 minutes;
[0058] (3) Hexadecyltrimethoxysilane is measured at a mass volume ratio of cotton fabric to hexadecyltrimethoxysilane of 1:60, and the cotton fabric treated in step (2) is added to the hexadecyltrimethoxysilane, reacted at 120° C. for 75 minutes, and then taken out, washed with a surfactant and deionized water, and then dried.
[0059] Example 3
[0060] (1) Take a clean cotton fabric and immerse it in a saturated copper ion solution of sodium hydroxide for 24 hours, wash it with deionized water until it is neutral, dry it and set it aside;
[0061] (2) preparing a 3% by mass solution of the gallnut extract, and immersing the cotton fabric treated in step (1) in the gallnut extract solution for 30 minutes;
[0062] (3) Hexadecyltrimethoxysilane is measured at a mass volume ratio of cotton fabric to hexadecyltrimethoxysilane of 1:70, and the cotton fabric treated in step (2) is added to the hexadecyltrimethoxysilane, reacted at 140° C. for 60 minutes, and then taken out, washed with a surfactant and deionized water, and then dried.
[0063] Example 4
[0064] (1) Take a clean cotton fabric and immerse it in a saturated copper ion solution of sodium hydroxide for 24 hours, wash it with deionized water until it is neutral, dry it and set it aside;
[0065] (2) preparing a 4% by mass solution of the gallnut extract, and immersing the cotton fabric treated in step (1) in the gallnut extract solution for 40 minutes;
[0066] (3) Hexadecyltrimethoxysilane is measured at a mass volume ratio of cotton fabric to hexadecyltrimethoxysilane of 1:80, and the cotton fabric treated in step (2) is added to the hexadecyltrimethoxysilane, reacted at 160° C. for 50 minutes, and then taken out, washed with a surfactant and deionized water, and then dried.
[0067] Example 5
[0068] (1) Take a clean cotton fabric and immerse it in a saturated copper ion solution of sodium hydroxide for 24 hours, wash it with deionized water until it is neutral, dry it and set it aside;
[0069] (2) preparing a 5% by mass solution of the gallnut extract, and immersing the cotton fabric treated in step (1) in the gallnut extract solution for 60 minutes;
[0070] (3) Hexadecyltrimethoxysilane is measured at a mass volume ratio of cotton fabric to hexadecyltrimethoxysilane of 1:120, and the cotton fabric treated in step (2) is added to the hexadecyltrimethoxysilane, reacted at 200° C. for 20 minutes, and then taken out, washed with a surfactant and deionized water, and then dried.
[0071] Example 6
[0072] (1) Take a clean cotton fabric and immerse it in a saturated copper ion solution of sodium hydroxide for 24 hours, wash it with deionized water until it is neutral, dry it and set it aside;
[0073] (2) preparing a glucose solution with a mass fraction of 2%, and immersing the cotton fabric treated in step (1) in the glucose solution for 20 minutes;
[0074] (3) Hexadecyltrimethoxysilane is measured according to a mass volume ratio of cotton fabric to hexadecyltrimethoxysilane of 1:100, and the cotton fabric treated in step (2) is added to the hexadecyltrimethoxysilane, reacted at 180° C. for 40 minutes, and then taken out, washed with a surfactant and dried.
[0075] Example 7
[0076] (1) Take a clean cotton fabric and immerse it in a saturated copper ion solution of sodium hydroxide for 24 hours, wash it with deionized water until it is neutral, dry it and set it aside;
[0077] (2) preparing a 2% by mass solution of honeysuckle extract, and immersing the cotton fabric treated in step (1) in the solution of honeysuckle extract for 20 minutes;
[0078] (3) Hexadecyltrimethoxysilane is measured according to a mass volume ratio of cotton fabric to hexadecyltrimethoxysilane of 1:100, and the cotton fabric treated in step (2) is added to the hexadecyltrimethoxysilane, reacted at 180° C. for 40 minutes, and then taken out, washed with a surfactant and dried.
[0079] Contact angle test: The contact angle test was performed using an OCA40 video contact angle meter produced by Dataphysics of Germany. The water volume was 5 μL and the reading was taken after the water droplet was in contact with the cotton fabric for 5 seconds. The same sample was measured 3 times at different locations and the average value was taken.
[0080] Antibacterial performance test: refer to GB / T20944.3-2008 "Evaluation of antibacterial properties of textiles Part 3: Oscillation method" to determine the antibacterial properties of the finished fabric.
[0081] from Figure 1 It can be seen that Example 1, Example 6, and Example 7 are darker in color due to cuprous oxide, Comparative Example 1-1 and Comparative Example 1-4 are blue due to copper ions, Comparative Example 1-2 is nearly colorless without adsorbing copper ions, and Comparative Example 1-3 is lighter in color, indicating that less copper ions are adsorbed.
[0082] from Figure 2 It can be seen that the XRD pattern of Example 1 shows diffraction peaks at 36.4°, 42.3°, 61.4° and 73.5°, corresponding to the (111), (200), (220) and (311) crystal planes of cuprous oxide, respectively, which proves that the copper ions inside the cellulose are successfully converted into cuprous oxide.
[0083] from Figure 3 It can be seen that the cotton fabrics prepared in Examples 1-7 have good hydrophobic properties, while Comparative Example 4 is hydrophilic because it is not hydrophobically modified by hexadecyltrimethoxysilane. Compared with the Examples, the hydrophobic properties of the Comparative Examples are poor.
[0084] from Figure 4 It can be seen that Comparative Example 1-2 did not adsorb copper ions, and the resulting cotton fabric had almost no antibacterial effect; Comparative Example 1-3 copper ions were only adsorbed on the surface of the cotton fabric, and during the subsequent washing process, cuprous oxide particles fell off, resulting in poor antibacterial effect. The antibacterial effect of Comparative Example 1-1 on Candida albicans was significantly worse than that of Example 1; although Comparative Example 1-4 had an antibacterial effect similar to that of Example 1, its water contact angle was 0°, showing hydrophilicity.
[0085] The invention adopts a saturated copper ion solution of sodium hydroxide to pretreat cotton fabric, and the copper ions are infiltrated into the interior of cotton fibers at the molecular level, coordinated with hydroxyl groups on the fibers, and stably combined in a cellulose matrix; subsequently, the cotton fabric absorbs a reducing agent and is immersed in hexadecyltrimethoxysilane, and at a high temperature, the reducing agent reduces the copper ions in the cellulose to cuprous oxide particles, and the hexadecyltrimethoxysilane provides a large amount of heat at a high temperature to promote the reaction, and reacts with a trace amount of water absorbed on the fibers to form Si-OH, and further condenses with the hydroxyl groups on the cellulose, thereby giving the cotton fabric excellent hydrophobicity.
[0086] It should be noted that the above embodiments are only used to illustrate the technical solutions of the present invention rather than to limit it. Although the present invention has been described in detail with reference to the preferred embodiments, those skilled in the art should understand that the technical solutions of the present invention can be modified or replaced by equivalents without departing from the spirit and scope of the technical solutions of the present invention, which should all be included in the scope of the present invention.
Claims
1. A method for preparing an antibacterial hydrophobic textile, characterized in that: include, A sodium hydroxide solution and a copper sulfate solution are prepared respectively, and the copper sulfate solution is added to the sodium hydroxide solution under stirring to obtain a saturated copper ion solution of sodium hydroxide; The dry cotton fabric is immersed in a saturated copper ion solution of sodium hydroxide at room temperature for 12 to 24 hours, the cotton fabric is taken out, the sodium hydroxide on the surface of the cotton fabric is washed off with clean water, and the cotton fabric is dried at room temperature to obtain a pretreated cotton fabric; The pretreated cotton fabric is immersed in a reducing agent solution at room temperature to obtain a reducing agent-treated cotton fabric; The cotton fabric treated with the reducing agent is mixed with hexadecyltrimethoxysilane, reacted at high temperature, washed with clean water, and dried to obtain the antibacterial and hydrophobic textile.
2. The preparation method according to claim 1, characterized in that: The concentration of the sodium hydroxide solution is 15 wt %.
3. The preparation method according to claim 1 or 2, characterized in that: The concentration of the copper sulfate solution is 0.02 mol / L.
4. The preparation method according to claim 3, characterized in that: The mixing volume ratio of the sodium hydroxide solution to the copper sulfate solution is 1:
1.
5. The preparation method according to claim 1, characterized in that: The dry cotton fabric is immersed in a saturated copper ion solution of sodium hydroxide at a bath ratio of 1:
100.
6. The preparation method according to claim 1, characterized in that: The reducing agent solution comprises one of a gallnut extract solution, a honeysuckle extract solution and a glucose solution, and the mass fraction thereof is 1% to 5%.
7. The preparation method according to claim 6, characterized in that: The pretreated cotton fabric is immersed in a reducing agent solution, wherein the bath ratio is 1:50 and the immersion time is 10 to 60 minutes.
8. The preparation method according to claim 1, characterized in that: The reducing agent-treated cotton fabric is mixed with hexadecyltrimethoxysilane, wherein the mass volume ratio of the cotton fabric to the hexadecyltrimethoxysilane is 1:60 to 1:120 g / mL.
9. The preparation method according to claim 8, characterized in that: The high temperature reaction, wherein the reaction temperature is 120-200° C., and the reaction time is 20-75 minutes.
10. The antibacterial and hydrophobic textile produced by the method according to any one of claims 1 to 9.