High-conductivity graphene / carbon cloth electrode material and preparation method thereof

By growing graphene in situ on the surface of carbon fiber, the problem of insufficient conductivity of carbon fiber cloth is solved, and high conductivity, lightweight and high flexibility electrode materials are achieved. It combines high conductivity and mechanical strength to be suitable for the integration of composite material structures. Avoid material damage.

CN119083157APending Publication Date: 2024-12-06NORTHWESTERN POLYTECHNICAL UNIV
View PDF 2 Cites 0 Cited by

Patent Information

Application Number
CN202411373290.4
Authority / Receiving Office
CN · China
Patent Type
Applications(China)
Current Assignee / Owner
Filing Date
2024-09-29
Publication Date
2024-12-06

AI Technical Summary

Technical Problem

The lack of conductivity of carbon fiber cloth as an electrode material leads to problems such as large resistance and large energy loss in high power density applications. Moreover, the interface bonding strength between graphene and carbon fiber matrix is ​​poor, which is easy to fall off, affecting mechanical properties.

Method used

Graphene is grown in situ on the surface of carbon fibers by low-pressure chemical vapor deposition, and methanol is used as a precursor to generate a highly conductive and thin-layer graphene sheet layer, which improves the conductivity of carbon fibers and enhances the bonding strength with carbon fibers.

Benefits of technology

It realizes high conductivity, lightweight, and highly flexible carbon cloth electrode materials, reduces the resistivity of carbon fibers, maintains mechanical strength and porous structure, is suitable for integration with composite material structure, and avoids mismatch of modulus and thermal expansion coefficient. 的材料破坏。

✦ Generated by Eureka AI based on patent content.

Smart Images

  • Figure CN119083157A_ABST
    Figure CN119083157A_ABST
Patent Text Reader

Abstract

The invention belongs to the field of electrode materials, and discloses a high-conductivity graphene / carbon cloth electrode material and a preparation method thereof.The electrode material comprises carbon fiber cloth and graphene growing on the fiber surface of the carbon fiber cloth in situ, and the graphene directly grows on the carbon fiber surface in situ through chemical vapor deposition; and the electrode material with high conductivity is prepared. The obtained electrode material retains the porous structure characteristics and good mechanical properties of the carbon cloth, can be applied to the fields of flexible electrodes, conductive fiber composite materials, electric heating ice prevention and removal and the like, and has wide application prospects and market potential.
Need to check novelty before this filing date? Find Prior Art

Description

Technical Field

[0001] The invention belongs to the field of electrode materials, and in particular relates to a highly conductive graphene / carbon cloth electrode material and a preparation method thereof. Background Art

[0002] In many industrial fields such as aviation, aerospace, and wind power, resin-based composite materials are often used as anti-icing structures, and the electrode materials commonly used are metal or graphite. However, the thermophysical properties and mechanical properties of these electrode materials are very different from those of resin-based composite materials, especially in terms of modulus and thermal expansion coefficient. This makes it easy for them to become defects during use as electrode materials, causing stress concentration and damage to the electric heating structure.

[0003] Using carbon fiber as an electrode material for conductive and electrothermal devices in composite materials is a way to solve the problem of mismatch between the mechanical and thermophysical properties of the electrode material and the device in the composite material. Because of its high specific strength and specific modulus, as well as the inherent electrochemical stability, corrosion resistance and high temperature resistance of carbon materials, it plays an important role in many fields such as aviation, aerospace, transportation, construction, and chemical industry. Carbon fiber mainly includes polyacrylonitrile-based or asphalt-based carbon fiber, which has a certain conductivity, but its conductivity still does not meet the requirements of electrode materials for high power density applications, and there are problems such as high resistance and high energy loss. Therefore, improving the conductivity of carbon fiber has become a key issue that needs to be solved.

[0004] Introducing graphene coating is an effective method to increase the conductivity of fiber electrode materials. The Chinese patent with publication number CN110931270A introduces a method for preparing graphene-based electrode fibers, using graphene dispersion as raw material and then coating graphene oxide on a metal fiber substrate with a diameter of 0.050.5 mm by alternating impregnation, and then obtaining graphene sheets by chemical reduction or thermal reduction, thereby obtaining a graphene-modified fiber electrode material with good mechanical properties and conductive properties. However, compared with metal fibers, the surface of carbon fibers has high chemical stability and low surface activity, and it is difficult to composite with other materials. Therefore, the interface bonding strength between the graphene obtained by the impregnation reduction method and the carbon fiber matrix is ​​poor, and it is easy to fall off and debond during use as an electrode; at the same time, the use of reducing agents will affect the structure of the carbon fiber itself, significantly reducing the mechanical strength of the carbon fiber. The Chinese patent with publication number CN117344531A uses plasma chemical vapor deposition to introduce oxygen-containing groups on the surface of carbon fiber, which can graft oxygen-containing functional groups without destroying the carbon fiber structure, and then react with graphene oxide to form a composite structure of graphene / carbon fiber soft felt. This method can reduce the resistance of carbon fiber to a certain extent, but the graphene layer is achieved by coating graphene oxide slurry, the coating thickness is large, the structure is loose, and it is not suitable for use occasions with high requirements for mechanical properties and power density. Summary of the invention

[0005] In view of the problem that the existing carbon fiber cloth has insufficient conductivity as an electrode material, the purpose of the present invention is to provide a highly conductive graphene / carbon cloth electrode material and a preparation method thereof. The present invention in situ grows graphene on the surface of carbon fiber to prepare a highly conductive carbon fiber cloth electrode material. In the electrode material, the graphene and the carbon fiber matrix are well combined, and the material has high conductivity, light weight and high flexibility. At the same time, the mechanical strength and porous structure of the carbon fiber cloth itself are retained, and the material is highly matched with the fiber-reinforced composite material structure, so that good integration with the composite material structure can be achieved.

[0006] To achieve the above object, the present invention adopts the following technical solution: A method for preparing a highly conductive graphene / carbon cloth electrode material comprises the following steps: Using methanol as a precursor and utilizing a low-pressure chemical vapor deposition method, graphene is in-situ grown on the fiber surface of the cleaned two-dimensional carbon fiber fabric to obtain the highly conductive graphene / carbon cloth electrode material.

[0007] Preferably, the cleaning process of the two-dimensional carbon fiber fabric comprises: soaking the two-dimensional carbon fiber fabric in an acetone solution, repeatedly cleaning it with deionized water and anhydrous ethanol alternately for several times, and then drying the water to complete the cleaning.

[0008] Preferably: the soaking time is 24 to 36 hours; Wash alternately with deionized water and anhydrous ethanol 3 to 5 times; The drying temperature is 75~85℃ and the drying time is 2~4h.

[0009] Preferably, when graphene is grown in situ on the fiber surface of the cleaned two-dimensional carbon fiber fabric using low-pressure chemical vapor deposition, the temperature is 800-1200°C.

[0010] Preferably, when graphene is grown in situ on the fiber surface of the cleaned two-dimensional carbon fiber fabric using low-pressure chemical vapor deposition, the pressure is 5-40 kPa.

[0011] Preferably, when graphene is grown in situ on the fiber surface of the cleaned two-dimensional carbon fiber fabric using low-pressure chemical vapor deposition, the deposition time is 5 min to 5 h.

[0012] Preferably, the fibers of the two-dimensional carbon fiber fabric are polyacrylonitrile-based or asphalt-based carbon fibers.

[0013] Preferably, the two-dimensional carbon fiber fabric is a non-woven, unidirectional non-woven, plain, or twill carbon fiber layer cloth.

[0014] The present invention also provides a highly conductive graphene / carbon cloth electrode material, which is prepared by the preparation method of the present invention as described above.

[0015] The present invention also provides the use of the highly conductive graphene / carbon cloth electrode material as described above, wherein the highly conductive graphene / carbon cloth electrode material is used for: Highly conductive flexible electrodes; Alternatively, it is compounded with a fiber composite material to prepare a conductive composite material structure comprising a graphene / carbon fiber cloth electrode; Or, as a highly conductive electrode material for the surface and internal electric heating elements of the composite material; Alternatively, highly conductive electrodes of composite materials can be prepared in the form of polymer-based prepregs.

[0016] The present invention has the following beneficial effects: In the present invention, only a single component of methanol is used as a precursor for direct reaction, and graphene is grown in situ on the fiber surface of the two-dimensional carbon fiber fabric. During the reaction, other reducing substances are generated by the cracking reaction of methanol to directly grow graphene, and other reducing agent substances are not added to participate in the reaction during the deposition process. Therefore, the present invention has low precursor cost, simple process, and good economic benefits. At the same time, the graphene sheets generated by the present invention have high compatibility and bonding strength with the fibers of the two-dimensional carbon fiber fabric, which solves the problem of powder loss and falling off of the graphene sheets during the use of the electrode; a very thin graphene sheet is in-situ grown on the fiber surface of the carbon cloth, and the resistivity of the carbon fiber is greatly reduced by utilizing the high conductivity of the graphene sheet and the high adhesion characteristics of the in-situ growth, thereby obtaining a highly conductive, lightweight and highly flexible carbon cloth electrode material; while graphene is in-situ grown on the carbon fiber surface, the mechanical strength and porous structure characteristics of the carbon fiber cloth itself are retained, and these characteristics make it highly compatible with the preparation processes of resin-based composite materials such as impregnation and hot pressing; the carbon fiber cloth structure with graphene in-situ grown on the surface has similar thermal physical properties and mechanical properties to the fiber structure of the composite material itself, thereby avoiding material damage caused by inconsistent modulus and thermal expansion coefficient of the electrode material. BRIEF DESCRIPTION OF THE DRAWINGS

[0017] Figure 1 This is a macroscopic morphology of an electrode material with graphene grown in situ on the surface of carbon cloth fibers prepared in Example 1 of the present invention; Figure 2 This is a microscopic morphology of the carbon fiber surface prepared in Example 1 of the present invention after in-situ growth of graphene; FIG3 (a) is a Braman spectrum of carbon fiber without graphene deposition in Example 1 of the present invention, and FIG3 (b) is a Braman spectrum of graphene / carbon fiber prepared in Example 1 of the present invention; Figure 4 It is a resistance comparison of the electrode samples prepared in the embodiments of the present invention.

[0018] FIG5(a) is an infrared analysis graph of the heating temperature of the electrode sample prepared in Example 1 of the present invention (modified with graphene) after applying a voltage of 25 V for 30 s; FIG5(b) is an infrared analysis graph of the heating temperature of the electrode sample prepared in Example 1 of the present invention (not modified with graphene) after applying a voltage of 255 V for 30 s.

[0019] Figure 6 are the temperature rise curves of the electrode samples prepared in Example 1 of the present invention at a voltage of 25 V; Figure 7 This is a schematic diagram of the structure of an electrothermal composite material including a high thermal conductivity carbon cloth electrode prepared in an example of the present invention.

[0020] FIG8 (a) is an infrared analysis graph of the heating temperature of the electrode sample prepared in Example 2 of the present invention (modified with graphene) after applying a voltage of 15 V for 30 s; FIG8 (b) is an infrared analysis graph of the heating temperature of the electrode sample prepared in Example 2 of the present invention (not modified with graphene) after applying a voltage of 15 V for 30 s; Fig. 9 are the temperature rise curves of the electrode samples prepared in Example 2 of the present invention at a voltage of 15 V; FIG10 (a) is an infrared analysis graph of the heating temperature of the electrode sample prepared in Example 3 of the present invention (modified with graphene) after applying a voltage of 20 V for 30 s; FIG10 (b) is an infrared analysis graph of the heating temperature of the electrode sample prepared in Example 3 of the present invention (not modified with graphene) after applying a voltage of 15 V for 30 s.

[0021] In the figure, 1-glass fiber cloth insulator, 2-high conductive graphene / carbon cloth electrode, 3-binary electric heating element. DETAILED DESCRIPTION

[0022] The specific implementation of the embodiment of the present invention is described in detail below in conjunction with the accompanying drawings. It should be understood that the specific implementation described here is only used to illustrate and explain the present invention, and is not used to limit the present invention.

[0023] The method for preparing the highly conductive graphene / carbon cloth electrode material of the present invention comprises the following steps: Step 1), cut the two-dimensional carbon fiber fabric into a desired shape, soak it in an acetone solution for 24 to 36 hours, and then wash it alternately with deionized water and anhydrous ethanol for 3 to 5 times, and then dry it at 75 to 85° C. for 2 to 4 hours to remove moisture for later use.

[0024] Step 2), using methanol as a precursor of graphene, using a low-pressure chemical vapor deposition system, at a temperature of 800-1200°C and a pressure of 5-40 kPa, chemical vapor deposition is performed to in-situ grow graphene on the fiber surface of the two-dimensional carbon fiber fabric obtained by treatment in step 1). The deposition time is controlled at 5 min-5 h, and then the introduction of the precursor is stopped. After the deposition furnace is cooled, the sample is taken out to complete the in-situ growth of graphene on the surface of the carbon fiber in the carbon cloth, and the highly conductive graphene / carbon cloth electrode material of the present invention is obtained.

[0025] In the above scheme of the present invention, methanol, as a precursor of graphene, is liquid at room temperature and can enter the chemical vapor deposition reaction chamber in gaseous form by heating to perform in-situ growth of graphene on the surface of carbon fiber.

[0026] In the present invention, the graphene deposition process can be controlled by adjusting the pressure and temperature.

[0027] The preparation method of the present invention solves the problem of insufficient conductivity of carbon cloth as an electrode material. By depositing graphene on the surface of carbon fiber, the conductivity of carbon fiber cloth is greatly improved, and the power consumption of carbon fiber cloth as an electrode material itself is reduced. The deposited graphene has good bonding strength with the carbon fiber in the carbon cloth, while maintaining the flexibility and porous characteristics of the carbon cloth, and highly matching the structure of the fiber-reinforced composite material. The carbon fiber in the two-dimensional carbon fiber fabric used has a certain conductivity itself, and the fibers in the two-dimensional carbon fiber fabric can be polyacrylonitrile-based or asphalt-based carbon fiber. The two-dimensional carbon fiber fabric can be any one or a combination of non-woven, unidirectional non-woven, plain, or twill carbon fiber layer cloth.

[0028] The highly conductive graphene / carbon cloth electrode material obtained by the above-mentioned preparation method of the present invention can be directly used as a highly conductive flexible electrode.

[0029] The highly conductive graphene / carbon cloth electrode material can also be compounded with a fiber composite material to replace a traditional copper electrode or a graphite electrode to prepare a conductive composite material structure containing a graphene / carbon fiber cloth electrode.

[0030] The highly conductive graphene / carbon cloth electrode material can also be used as a highly conductive electrode material for electric heating elements on the surface and inside of composite materials (such as carbon cloth heating elements or other fiber electric heating elements), and can be used for electric heating anti-icing of composite materials.

[0031] The highly conductive graphene / carbon cloth electrode material can also be used in the form of a polymer-based prepreg to prepare a highly conductive electrode of a composite material.

[0032] Embodiment 1: The method for preparing the highly conductive graphene / carbon cloth electrode material of this embodiment comprises the following steps: Step 1), the two-dimensional carbon fiber fabric is cut into a rectangular carbon cloth of 50 mm × 100 mm, then soaked in an acetone solution for 24 hours, taken out, washed with deionized water and anhydrous ethanol for 5 times, and dried at 75 ° C for use.

[0033] Step 2) Using methanol as a precursor, a vertical low-pressure chemical vapor deposition system is used to heat the methanol to a gaseous state and enter the chemical vapor deposition reaction chamber, and chemical vapor deposition is performed under the set conditions of 1000°C and 35 kPa to in-situ grow graphene on the fiber surface of the carbon cloth.

[0034] In step 3), the deposition time is controlled at 5 min, and then the introduction of the precursor is stopped. After the deposition furnace is cooled to room temperature, the electrode sample is taken out to complete the in-situ growth of graphene on the surface of the carbon fiber in the carbon cloth, and the highly conductive graphene / carbon cloth electrode material of this embodiment is obtained.

[0035] Depend on Figure 1 The figure shows the macroscopic morphology of the highly conductive graphene / carbon cloth electrode material prepared in this embodiment, wherein the fibers are continuous and the surface of the carbon cloth is intact. This complete structure is the basis for forming this highly conductive electrode material; Figure 2 Figure 3 is a microscopic morphology of the carbon fiber surface prepared in this example after in-situ growth of graphene. It can be seen that the graphene grows laterally along the fiber surface. This continuous and complete graphene structure is the main reason for improving the conductivity of the carbon fiber fabric. Figure 3 (a) and Figure 3 (b) are the Raman spectra tested. The D peak (1350 cm -1 ) represents turbostratic graphite or defects, and the G peak (1580 cm -1 ) represents graphitic carbon, which means that with the deposition of lamellar graphene on the surface of carbon fiber, its defects are reduced, and the crystallinity and graphitization degree are improved.

[0036] The resistance of the electrode sample obtained in step 3) is measured to be 0.4 Ω, while the resistance of the carbon cloth without graphene deposition (i.e., the carbon cloth obtained in step 1) is 11.2 Ω. In comparison, the resistivity of the highly conductive graphene / carbon cloth electrode material prepared in this embodiment is reduced by 96.4% relative to the resistivity of the original carbon cloth (i.e., the carbon cloth obtained in step 1), as shown in FIG. Figure 4 shown.

[0037] The electrode sample obtained in step 3) and the carbon cloth without graphene deposition (i.e. the carbon cloth obtained in step 1)) were used as electrodes, and the thermoelectric performance test was carried out under a DC voltage of 25V, and the operation was as follows: Pretreated glass fiber fabric was selected as the electric heating element (5-1000 Ω). First, carbon slurry was coated on the surface of the electric heating element, and after being bonded with the electrode sample obtained in step 3), it was placed at room temperature for 12 hours, and then placed in an 80°C oven for 6 hours, so that the electrode sample obtained in step 3) was connected to the conductive fiber fabric to obtain the first heating device. At the same time, the carbon cloth obtained in step 1) was used to replace the electrode sample obtained in step 3), and the second heating device was obtained in the same manner as above.

[0038] The first heating device and the second heating device were connected to a DC power supply and tested at a voltage of 25 V. The real-time temperature test was performed using an infrared thermometer. As shown in Figures 5 (a) and 5 (b), the heating temperature reached 118.2 °C after applying a voltage of 25 V for more than 30 s. Compared with the temperature of the carbon cloth electrode without graphene modification of 86.7 °C, the power loss was reduced from 0.0614 W to 0.0113 W. It can be concluded that the electrode prepared by depositing continuous and complete sheets of graphene on the surface of carbon fiber is well combined with the electric heating element. With the introduction of graphene, the conductivity of carbon fiber as an electrode can be effectively improved and energy consumption can be reduced. At the same time, Figure 6It can be seen from the heating curve that the carbon cloth electrode modified with graphene is easier to reach the heating limit temperature during the heating process than the carbon cloth electrode not modified with graphene.

[0039] Embodiment 2: The method for preparing the highly conductive graphene / carbon cloth electrode material of this embodiment comprises the following steps: Step 1), the two-dimensional carbon fiber fabric is cut into a rectangular carbon cloth of 50 mm × 100 mm, then immersed in an acetone solution for 30 h and taken out, washed with deionized water and anhydrous ethanol for 4 times, and dried at 85 °C for use.

[0040] Step 2) Using methanol as a precursor, a vertical low-pressure chemical vapor deposition system is used to heat the methanol to a gaseous state and enter the chemical vapor deposition reaction chamber, and chemical vapor deposition is performed under the setting conditions of 1100°C and 40kPa to in-situ grow graphene on the fiber surface of the carbon cloth.

[0041] In step 3), the deposition time is controlled at 5 h, and then the introduction of the precursor is stopped. After the deposition furnace is cooled to room temperature, the electrode sample is taken out to complete the in-situ growth of graphene on the surface of the carbon fiber in the carbon cloth, and the highly conductive graphene / carbon cloth electrode material of this embodiment is obtained.

[0042] The resistance of the electrode sample obtained in step 3) was measured to be 0.6 Ω, while the resistance of the carbon cloth without graphene deposition (i.e., the carbon cloth obtained in step 1) was 11.2 Ω. In comparison, the resistivity of the highly conductive graphene / carbon cloth electrode material prepared in this embodiment was reduced by 94.6% relative to the resistivity of the original carbon cloth (i.e., the carbon cloth obtained in step 1)).

[0043] The electrode sample obtained in step 3) is prepared into a composite material, and the operation is as follows: First, the electrode sample is placed in an acetone solution and soaked for 30 minutes, followed by ultrasonic dispersion; 50 g of epoxy resin is added to a beaker together with the electrode sample, and ultrasonic and mechanical stirring is performed for 1 hour to fully disperse the epoxy resin, and then the graphene / carbon fiber cloth prepreg is taken out and dried for standby use; the sample (i.e., graphene / carbon fiber cloth prepreg) is hot-pressed with the fiber electrothermal heating element and the glass fiber prepreg to obtain a composite material with integrated highly conductive graphene / carbon fiber cloth electrodes. The schematic diagram of the structural combination is shown in FIG. Figure 7 As shown, it includes a glass fiber cloth insulator, a two-dimensional electric heating element and a high thermal conductivity graphene / carbon cloth electrode.

[0044] The first heating device and the second heating device were connected to a DC power supply and tested at a voltage of 15 V. The real-time temperature test was performed using an infrared thermometer. As shown in Figures 8 (a) and 8 (b), the heating temperature reached 66.4 °C after applying a voltage of 15 V for more than 30 s. Compared with the temperature of the carbon cloth electrode without graphene modification at 48.5 °C, the power loss was reduced from 0.0187 W to 0.0036 W. Fig. 9 From the heating curve, it can be seen that the carbon cloth electrode modified with graphene is easier to reach the heating limit temperature during the heating process than the carbon cloth electrode not modified with graphene. This example proves that after using graphene-modified carbon cloth as the electrode material, the electrothermal performance of the composite material is still good, and the heating effect after applying direct current is significant.

[0045] Example 3 The method for preparing the highly conductive graphene / carbon cloth electrode material of this embodiment comprises the following steps: Step 1), the two-dimensional carbon fiber fabric is cut into a rectangular carbon cloth of 50 mm × 100 mm, then immersed in an acetone solution for 36 hours, taken out, washed with deionized water and anhydrous ethanol three times, and dried at 80°C for use.

[0046] Step 2) Using methanol as a precursor, a vertical low-pressure chemical vapor deposition system is used to heat the methanol to a gaseous state and enter the chemical vapor deposition reaction chamber, and chemical vapor deposition is performed under the set conditions of 800°C and 5 kPa to in-situ grow graphene on the fiber surface of the carbon cloth.

[0047] Step 3), the deposition time is controlled at 120 min, then the introduction of the precursor is stopped, and the electrode sample is taken out after the deposition furnace is cooled to room temperature, completing the in-situ growth of graphene on the surface of the carbon fiber in the carbon cloth, and obtaining the highly conductive graphene / carbon cloth electrode material of this embodiment.

[0048] The resistance of the electrode sample obtained in step 3) was measured to be 0.7 Ω, while the resistance of the carbon cloth without graphene deposition (i.e., the carbon cloth obtained in step 1) was 11.1 Ω. In comparison, the resistivity of the highly conductive graphene / carbon cloth electrode material prepared in this embodiment was reduced by 93.7% relative to the resistivity of the original carbon cloth (i.e., the carbon cloth obtained in step 1)).

[0049] The electrode sample obtained in step 3) and the carbon cloth without graphene deposition (i.e. the carbon cloth obtained in step 1)) were used as electrodes to perform thermoelectric performance tests at a DC voltage of 20V, respectively, as follows: Pretreated glass fiber fabric was selected as the electric heating element (5-1000 Ω). First, carbon slurry was coated on the surface of the electric heating element, and after being bonded with the electrode sample obtained in step 3), it was placed at room temperature for 12 hours, and then placed in an 80°C oven for 6 hours, so that the electrode sample obtained in step 3) was connected to the conductive fiber fabric to obtain the first heating device. At the same time, the carbon cloth obtained in step 1) was used to replace the electrode sample obtained in step 3), and the second heating device was obtained in the same manner as above.

[0050] The first heating device and the second heating device were connected to a DC power supply and tested at a voltage of 20 V. The real-time temperature test was performed by an infrared thermometer. As shown in Figures 10 (a) and 10 (b), the heating temperature reached 91.7 °C after applying a voltage of 20 V for more than 30 s. Compared with the temperature of the carbon cloth electrode without graphene modification of 62.5 °C, the power loss was reduced from 0.0425 W to 0.0109 W. Compared with Example 1, the power loss of the electrode prepared at 800 °C in Example 3 is larger.

[0051] It can be seen from the above technical scheme of the present invention that the present invention uses a methanol precursor and adopts a chemical vapor deposition method to directly grow graphene in situ on the surface of a carbon fiber cloth to prepare a highly conductive carbon cloth electrode material. The method has a simple process, low precursor cost, and the prepared graphene is well combined with the carbon fiber matrix, and has high conductivity, light weight, and high flexibility. At the same time, the mechanical strength and porous structure of the carbon fiber cloth itself are retained, and the structure is highly matched with the fiber-reinforced composite material, and a good integration with the composite material structure can be achieved.

[0052] Although the embodiments of the present invention have been disclosed as above, they are not limited to the applications listed in the specification and implementation modes. They can be fully applied to the fields suitable for the present invention. For those familiar with the art, additional modifications can be easily implemented. Therefore, without departing from the general concept defined by the equivalent scope of the claims, the present invention is not limited to the specific details and illustrations shown and described herein.

Claims

1. A method for preparing a highly conductive graphene / carbon cloth electrode material, characterized in that: The process includes the following: Using methanol as a precursor and utilizing a low-pressure chemical vapor deposition method, graphene is in-situ grown on the fiber surface of the cleaned two-dimensional carbon fiber fabric to obtain the highly conductive graphene / carbon cloth electrode material.

2. The method for preparing a highly conductive graphene / carbon cloth electrode material according to claim 1, characterized in that: The cleaning process of the two-dimensional carbon fiber fabric includes: soaking the two-dimensional carbon fiber fabric in an acetone solution, repeatedly cleaning it with deionized water and anhydrous ethanol for several times, and then drying the water to complete the cleaning.

3. The method for preparing a highly conductive graphene / carbon cloth electrode material according to claim 2, characterized in that: Soaking time is 24~36h; Wash alternately with deionized water and anhydrous ethanol 3 to 5 times; The drying temperature is 75~85℃ and the drying time is 2~4h.

4. The method for preparing a highly conductive graphene / carbon cloth electrode material according to claim 1, characterized in that: When graphene is grown in situ on the fiber surface of the cleaned two-dimensional carbon fiber fabric using low-pressure chemical vapor deposition, the temperature is 800~1200℃.

5. The method for preparing a highly conductive graphene / carbon cloth electrode material according to claim 1, characterized in that: When graphene is grown in situ on the fiber surface of the cleaned two-dimensional carbon fiber fabric using low-pressure chemical vapor deposition, the pressure is 5~40kPa.

6. The method for preparing a highly conductive graphene / carbon cloth electrode material according to claim 1, characterized in that: When graphene is grown in situ on the fiber surface of the cleaned two-dimensional carbon fiber fabric using low-pressure chemical vapor deposition, the deposition time is 5 minutes to 5 hours.

7. The method for preparing a highly conductive graphene / carbon cloth electrode material according to claim 1, characterized in that: The fibers of the two-dimensional carbon fiber fabric are polyacrylonitrile-based or asphalt-based carbon fibers.

8. The method for preparing a highly conductive graphene / carbon cloth electrode material according to claim 1, characterized in that: Two-dimensional carbon fiber fabrics use non-woven, unidirectional non-woven, plain, or twill carbon fiber layers.

9. A highly conductive graphene / carbon cloth electrode material, characterized in that: The highly conductive graphene / carbon cloth electrode material is prepared by the preparation method according to any one of claims 1 to 8.

10. The use of the highly conductive graphene / carbon cloth electrode material according to claim 9, characterized in that: The highly conductive graphene / carbon cloth electrode material is used for: Highly conductive flexible electrodes; Alternatively, it is compounded with a fiber composite material to prepare a conductive composite material structure comprising a graphene / carbon fiber cloth electrode; Or, as a highly conductive electrode material for the surface and internal electric heating elements of the composite material; Alternatively, highly conductive electrodes of composite materials can be prepared in the form of polymer-based prepregs.

Citation Information

Patent Citations

  • Preparation method of graphene-based electrode fiber containing substrate

    CN110931270A

  • Electrode soft felt preparation method based on pre-oxidized carbon fiber composite graphene, electrode soft felt and battery